Method for producing activated zinc oxide by wet process

Through the improved wet process, precipitants such as dodecylbenzenesulfonic acid, hydrogen peroxide and modified graphene combined with sodium carbonate medium, the influence of impurity ions in wet zinc oxide recovery was solved and the purity of zinc oxide was improved. It also reduces the content of impurity elements and realizes the production of high-purity zinc oxide.

CN118908267AActive Publication Date: 2024-11-08ZHUZHOU ANTE NEW MATERIAL TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411049302.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-08
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The existing wet zinc oxide recovery process is prone to introduce impurity ions, affecting the purity of zinc oxide. In addition, the traditional zinc powder reduction and impurity removal process is not effective at low heavy metal ion concentrations, making it difficult to further reduce the content of impurity elements.

Method used

A method of producing active zinc oxide by wet method, by soaking the zinc-containing furnace tailslag mill powder in a sulfuric acid solution, and then adding a mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide to form iron ions and use modification Precipitant treatment is carried out by precipitation, and finally calcined under sodium carbonate medium to form active zinc oxide, which reduces the content of impurity elements through selective adsorption and ion exchange of the precipitant.

Benefits of technology

The purity of zinc oxide is improved, the requirements of high-purity active zinc oxide are met, and the content of impurities in the product is further reduced based on traditional processes, especially at low concentrations to effectively remove lead and cadmium ions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004974436950000141
    Figure BDA0004974436950000141
Patent Text Reader

Abstract

The invention discloses a method for producing activated zinc oxide by a wet process, which comprises the following steps: (1) leaching zinc-containing furnace tailings in a sulfuric acid solution to obtain a leaching solution; (2) oxidizing, namely oxidizing ferrous ions to form iron ions; (3) preparing a precipitator; removing impurities to obtain zinc-containing liquid; and (4) adding sodium carbonate into the zinc-containing liquid to obtain basic zinc carbonate precipitate, carrying out solid-liquid separation, and then calcining and decomposing to generate the activated zinc oxide. The product zinc oxide obtained by adopting the method disclosed by the invention is relatively high in purity, and meets the requirements on high-purity activated zinc oxide. A novel precipitator is introduced on the basis of a traditional zinc powder reduction impurity removal process, and the content of impurity elements in the product is further reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of zinc oxide recovery, and in particular to a method for producing active zinc oxide by a wet process. Background Art

[0002] Active zinc oxide is a commonly used chemical additive with a wide range of uses. It is mainly used as a raw material in industries such as rubber, coatings, printing and dyeing, feed, medicine, chemicals and ceramics. Active zinc oxide is used as a reinforcing agent, colorant, vulcanizer and compounding agent for increasing thermal conductivity in the rubber industry; in the coating industry, it is mainly used for its tinting power, hiding power, anti-corrosion, luminescence and other functions; in the printing and dyeing industry, it is used as a dye resist; in the feed industry, it is used as a feed additive. In addition, active zinc oxide is also used as a raw material for producing opalescent glass, zinc white oil paint and watercolor pigments, as well as cosmetics and various zinc salts. There are two methods for industrial production of zinc oxide: dry method and wet method. The dry method includes direct method and indirect method. The direct method uses smithsonite, zinc sulfide ore, sphalerite, subzinc oxide ore and the like as raw materials, adds a reducing agent, and directly calcines the zinc vapor produced at high temperature to contact with hot air for oxidation to generate zinc oxide. The product quality is relatively unstable; the indirect method is to first refine the zinc ore into zinc ingots, and then use the zinc ingots to produce zinc oxide. The cost of this method is too high and its development is restricted. The wet treatment process includes leaching, electrolysis, deposition and other processes. Since zinc oxide is an amphoteric oxide, both acid and alkali can be used to extract and recover zinc oxide. However, the commonly used recovery process is prone to introduce new impurity ions, such as chloride ions, sodium ions, etc., which affect the purity of zinc oxide. Summary of the invention

[0003] To this end, the present invention provides a method for producing active zinc oxide by a wet process, the steps comprising:

[0004] (1) Grind the zinc-containing furnace tailings into powder, soak the powder in a sulfuric acid solution, heat it in a water bath to 55±5°C, keep it warm and stir it for more than 1 hour, then air cool it to room temperature, separate the solid and liquid, and obtain a leachate;

[0005] (2) preparing a mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide; stirring the leachate, and then adding the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide to the leachate under stirring to obtain a mixed solution, and continuing to stir the mixed solution for more than 30 minutes after the addition is completed to oxidize the ferrous ions to form ferric ions;

[0006] (3) preparing a precipitant; stirring the mixed solution, then adding the precipitant to the mixed solution under stirring, heating the mixed solution to 50±5° C. in a water bath and stirring for more than 20 minutes, then separating the solid and the liquid to obtain a filtrate and a filter residue, soaking the filter residue in a dilute hydrochloric acid solution and ultrasonically vibrating for more than 10 minutes, then separating the solid and the liquid, washing the solid phase with deionized water until the washed solution is neutral, then soaking the solid phase in the filtrate again, heating the mixed solution to 50±5° C. in a water bath and stirring for more than 20 minutes, and then separating the solid and the liquid after the insulation to obtain a zinc-containing liquid;

[0007] (4) adding sodium carbonate to the zinc-containing solution, heating in a water bath to 60±5° C. and stirring for more than 1 hour to obtain basic zinc carbonate precipitate, separating the solid from the liquid, washing the solid phase with deionized water for more than 3 times, and then calcining and decomposing to generate the active zinc oxide;

[0008] The preparation method of the precipitant is as follows:

[0009] Step 1, preparing an aqueous solution of sodium hydroxide; adding graphene oxide to the aqueous solution of sodium hydroxide, stirring for more than 30 minutes, then adding carbon disulfide to the solution under stirring, stirring for more than 20 minutes after the addition is completed, and then heating in a water bath to 40±3°C and stirring for more than 5 hours, separating the solid and the liquid after the insulation is completed, washing the solid phase with ethanol for more than 3 times, and then washing with deionized water for more than 3 times, and drying at 40°C for more than 20 hours to obtain modified graphene;

[0010] Step 2, prepare an aqueous solution of ethanol; prepare a mixed aqueous solution of acrylamide and acrylic acid; add the modified graphene to the aqueous solution of ethanol, stir and disperse for more than 30 minutes under an ultrasonic environment to obtain a dispersion, then add γ-methacryloxypropyltrimethoxysilane to the dispersion under stirring, adjust the pH to 4 with hydrochloric acid after the addition is completed, then heat to 50±3°C in a water bath in an argon protective atmosphere and stir for more than 3 hours, then separate the solid and liquid, wash the solid phase with ethanol for more than 3 times, dry at 40°C for more than 20 hours, add the solid phase to the mixed aqueous solution of acrylamide and acrylic acid after drying, stir for more than 20 minutes after the addition, then add N,N-methylenebisacrylamide to the solution under stirring, continue to stir for more than 20 minutes after the addition is completed, then place the mixed solution in an argon protective atmosphere, heat to 60±3°C in a water bath and keep warm, then add the initiator, and after the addition is completed, keep warm and stir at 60±3°C in an argon atmosphere for more than 2 hours,

[0011] Then the solid and liquid are separated, the solid phase is washed with ethanol for more than 2 times, and then washed with deionized water for more than 2 times, and dried at 50°C for more than 10 hours. The dried solid phase is evenly mixed with zinc powder passed through a 1000-mesh sieve, and the mass ratio of the dried solid phase to the zinc powder is the dried solid phase: zinc powder = 1:3, to obtain the precipitant.

[0012] Furthermore, in the step (1), the mass percentage of the solute in the sulfuric acid solution is 30%, and the solid-liquid mass ratio of the powder immersed in the sulfuric acid solution is powder: sulfuric acid solution = 1:10.

[0013] Furthermore, in the step (2), in the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide, the mass percentage of H2O2 is 20%, the mass percentage of dodecylbenzenesulfonic acid is 2% to 3%, and the solvent is water; the volume ratio of the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide added to the leachate is leachate: mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide = 10:3 to 4.

[0014] Furthermore, in the step (3), the mass ratio of the precipitant added to the mixed solution is mixed solution:precipitant=10:1-3.

[0015] Furthermore, in the step (4), the mass ratio of sodium carbonate added to the zinc-containing liquid is zinc-containing liquid: sodium carbonate = 100:10-14; the calcination temperature is 800° C., and the calcination time is 1 hour.

[0016] Furthermore, in the step 1, the concentration of sodium hydroxide in the aqueous solution of sodium hydroxide is 10-12 g / 100 mL, and the solvent is water; the mass ratio of the added mass of graphene oxide and carbon disulfide to the aqueous solution of sodium hydroxide is graphene oxide: carbon disulfide: aqueous solution of sodium hydroxide = 3-4:6-7:100.

[0017] Further, in the step 2, the volume percentage of ethanol in the ethanol aqueous solution is 60%; in the mixed aqueous solution of acrylamide and acrylic acid, the concentration of acrylamide is 4.2-4.6 g / 100 mL, the concentration of acrylic acid is 1.7-2.5 g / 100 mL, and the solvent is water; the solid-liquid mass ratio of the modified graphene added to the ethanol aqueous solution is modified graphene: ethanol aqueous solution = 1:50; the mass ratio of the added mass of γ-methacryloxypropyltrimethoxysilane to the mass of the modified graphene in the dispersion is γ-methacryloxypropyltrimethoxysilane. The mass ratio of the dried solid phase added to the mixed aqueous solution of acrylamide and acrylic acid is solid phase after drying: mixed aqueous solution of acrylamide and acrylic acid is 1:80, the mass ratio of the added mass of N,N-methylenebisacrylamide and initiator to the mass ratio of the dried solid phase added to the mixed aqueous solution of acrylamide and acrylic acid is N,N-methylenebisacrylamide: initiator: dried solid phase = 1.2-1.6:0.2-0.3:1; the initiator is ammonium persulfate.

[0018] The beneficial effect of the present invention is that the product zinc oxide obtained by the method of the present invention has high purity and meets the requirements for high-purity active zinc oxide. The present invention introduces a new precipitant based on the traditional zinc powder reduction and impurity removal process, further reducing the content of impurity elements in the product. DETAILED DESCRIPTION

[0019] The present invention will be further described below in conjunction with the embodiments.

[0020] Example 1

[0021] A method for producing active zinc oxide by a wet process, comprising the steps of:

[0022] (1) Grinding zinc-containing furnace tailings (the main chemical composition analysis results are shown in Table 1) into powder, and soaking the powder in a sulfuric acid solution, wherein the mass ratio of the solute in the sulfuric acid solution is 30%, and the solid-liquid mass ratio of the powder soaked in the sulfuric acid solution is powder: sulfuric acid solution = 1:10; heating in a water bath to 55±5°C, keeping the temperature and stirring for 1h, and then air cooling to room temperature, solid-liquid separation, and obtaining a leachate;

[0023] (2) preparing a mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide; in the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide, the mass percentage of H2O2 is 20%, the mass percentage of dodecylbenzenesulfonic acid is 2%, and the solvent is water; stirring the leachate, and then adding the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide to the leachate under stirring to obtain a mixed solution, wherein the volume ratio of the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide added to the leachate is leachate: mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide = 10:3; after the addition is completed, continuing to stir the mixed solution for 30 minutes to oxidize the ferrous ions to form ferric ions;

[0024] (3) preparing a precipitant; stirring the mixed solution, and then adding the precipitant to the mixed solution under stirring, wherein the mass ratio of the precipitant added to the mixed solution is mixed solution: precipitant = 10:1; heating the mixed solution in a water bath to 50±5° C. and stirring for 20 min, and then performing solid-liquid separation to obtain a filtrate and a filter residue, soaking the filter residue in a dilute hydrochloric acid solution (5% by mass of the solute) and performing ultrasonic vibration for 10 min, performing a reactivation treatment on the precipitant, removing adsorbed lead and cadmium ions, and then performing solid-liquid separation, washing the solid phase with deionized water until the washed solution is neutral, and then soaking the solid phase in the filtrate again, heating the mixed solution in a water bath to 50±5° C. and stirring for 20 min, and then performing solid-liquid separation after the insulation to obtain a zinc-containing liquid;

[0025] (4) adding sodium carbonate to the zinc-containing solution, wherein the mass ratio of sodium carbonate to the zinc-containing solution is zinc-containing solution: sodium carbonate = 100:10; heating in a water bath to 60±5° C. and stirring for 1 hour to obtain basic zinc carbonate precipitate, separating the solid from the liquid, washing the solid phase with deionized water for 3 times, and then calcining and decomposing the precipitate at a calcination temperature of 800° C. for 1 hour to generate the active zinc oxide;

[0026] The preparation method of the precipitant is as follows:

[0027] Step 1, prepare an aqueous solution of sodium hydroxide; in the aqueous solution of sodium hydroxide, the concentration of sodium hydroxide is 10g / 100mL, and the solvent is water; add graphene oxide to the aqueous solution of sodium hydroxide, stir for 30min, and then add carbon disulfide to the solution under stirring, the mass ratio of graphene oxide and carbon disulfide added to the aqueous solution of sodium hydroxide is graphene oxide: carbon disulfide: aqueous solution of sodium hydroxide = 3:6:100; after the addition is completed, stir for 20min, then heat in a water bath to 40±3°C and keep stirring for 5h, separate the solid and liquid after the insulation is completed, wash the solid phase with ethanol 3 times, then wash with deionized water 3 times, and dry at 40°C for 20h to obtain modified graphene;

[0028] Step 2, preparing an aqueous solution of ethanol; the volume percentage of ethanol in the aqueous solution of ethanol is 60%; preparing a mixed aqueous solution of acrylamide and acrylic acid; in the mixed aqueous solution of acrylamide and acrylic acid, the concentration of acrylamide is 4.2g / 100mL, the concentration of acrylic acid is 1.7g / 100mL, and the solvent is water; adding the modified graphene to the aqueous solution of ethanol, the solid-liquid mass ratio of the modified graphene added to the aqueous solution of ethanol is modified graphene: ethanol aqueous solution = 1:50; stirring and dispersing under an ultrasonic environment for 30 minutes to obtain dispersion, and then adding γ-methacryloxypropyltrimethoxysilane to the dispersion under stirring, the mass ratio of the added mass of γ-methacryloxypropyltrimethoxysilane to the modified graphene in the dispersion is γ-methacryloxypropyltrimethoxysilane: modified graphene = 2:1; after the addition is completed, the pH is adjusted to 4 with hydrochloric acid (the mass percentage of the solute is 20%), and then heated to 50±3°C in a water bath in an argon protective atmosphere and stirred for 3h, and then the solid-liquid separation is carried out, the solid phase is washed 3 times with ethanol, and dried at 40°C for 20h, and dried The solid phase after drying is added to the mixed aqueous solution of acrylamide and acrylic acid, and the solid-liquid mass ratio of the solid phase after drying to the mixed aqueous solution of acrylamide and acrylic acid is the solid phase after drying: the mixed aqueous solution of acrylamide and acrylic acid = 1:80. After adding, stir for 20 minutes, and then add N, N-methylenebisacrylamide to the solution under stirring. After the addition is completed, continue to stir for 20 minutes, and then place the mixed solution in an argon protection atmosphere, heat it in a water bath to 60 ± 3 ° C for insulation, and then add the initiator. The added mass of the N, N-methylenebisacrylamide and the initiator is the same as that of the initiator. The mass ratio of the dried solid phase added to the mixed aqueous solution of acrylamide and acrylic acid is N,N-methylenebisacrylamide:initiator:dried solid phase=1.2:0.2:1; the initiator is ammonium persulfate; after the addition is completed, the mixture is kept warm and stirred at 60±3°C in an argon atmosphere for 2 hours, then the solid and liquid are separated, the solid phase is washed twice with ethanol, then washed twice with deionized water, and dried at 50°C for 10 hours, the dried solid phase is evenly mixed with zinc powder passed through a 1000-mesh sieve, and the mass ratio of the dried solid phase to the zinc powder is dried solid phase: zinc powder=1:3, to obtain the precipitant.

[0029] Example 2

[0030] A method for producing active zinc oxide by a wet process, comprising the steps of:

[0031] (1) Grinding zinc-containing furnace tailings (the main chemical composition analysis results are shown in Table 1) into powder, and soaking the powder in a sulfuric acid solution, wherein the mass ratio of the solute in the sulfuric acid solution is 30%, and the solid-liquid mass ratio of the powder soaked in the sulfuric acid solution is powder: sulfuric acid solution = 1:10; heating in a water bath to 55±5°C, keeping the temperature and stirring for 1h, and then air cooling to room temperature, solid-liquid separation, and obtaining a leachate;

[0032] (2) preparing a mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide; in the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide, the mass percentage of H2O2 is 20%, the mass percentage of dodecylbenzenesulfonic acid is 2%, and the solvent is water; stirring the leachate, and then adding the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide to the leachate under stirring to obtain a mixed solution, wherein the volume ratio of the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide added to the leachate is leachate: mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide = 10:3; after the addition is completed, continuing to stir the mixed solution for 30 minutes to oxidize the ferrous ions to form ferric ions;

[0033] (3) preparing a precipitant; stirring the mixed solution, and then adding the precipitant to the mixed solution under stirring, wherein the mass ratio of the precipitant added to the mixed solution is mixed solution: precipitant = 10:2; heating the mixture to 50±5° C. in a water bath and stirring for 20 min, then performing solid-liquid separation to obtain a filtrate and a filter residue, soaking the filter residue in a dilute hydrochloric acid solution (5% by mass of the solute) and performing ultrasonic vibration for 10 min, performing a reactivation treatment on the precipitant, removing adsorbed lead and cadmium ions, then performing solid-liquid separation, washing the solid phase with deionized water until the washed solution is neutral, then soaking the solid phase in the filtrate again, heating the mixture to 50±5° C. in a water bath and stirring for 20 min, and performing solid-liquid separation after the insulation to obtain a zinc-containing liquid;

[0034] (4) adding sodium carbonate to the zinc-containing solution, wherein the mass ratio of sodium carbonate to the zinc-containing solution is zinc-containing solution: sodium carbonate = 100:12; heating in a water bath to 60±5° C. and stirring for 1 h to obtain basic zinc carbonate precipitate, separating the solid from the liquid, washing the solid phase with deionized water for 3 times, and then calcining and decomposing the precipitate at a calcination temperature of 800° C. for 1 h to generate the active zinc oxide;

[0035] The preparation method of the precipitant is as follows:

[0036] Step 1, prepare an aqueous solution of sodium hydroxide; in the aqueous solution of sodium hydroxide, the concentration of sodium hydroxide is 11g / 100mL, and the solvent is water; add graphene oxide to the aqueous solution of sodium hydroxide, stir for 30min, and then add carbon disulfide to the solution under stirring, the mass ratio of graphene oxide and carbon disulfide added to the aqueous solution of sodium hydroxide is graphene oxide: carbon disulfide: aqueous solution of sodium hydroxide = 3:6:100; after the addition is completed, stir for 20min, then heat in a water bath to 40±3°C and keep stirring for 5h, separate the solid and liquid after the insulation is completed, wash the solid phase with ethanol 3 times, then wash with deionized water 3 times, and dry at 40°C for 20h to obtain modified graphene;

[0037] Step 2, preparing an aqueous solution of ethanol; the volume percentage of ethanol in the aqueous solution of ethanol is 60%; preparing a mixed aqueous solution of acrylamide and acrylic acid; in the mixed aqueous solution of acrylamide and acrylic acid, the concentration of acrylamide is 4.4g / 100mL, the concentration of acrylic acid is 2g / 100mL, and the solvent is water; adding the modified graphene to the aqueous solution of ethanol, the solid-liquid mass ratio of the modified graphene added to the aqueous solution of ethanol is modified graphene: ethanol aqueous solution = 1:50; stirring and dispersing for 30min under an ultrasonic environment to obtain a dispersed liquid, and then add γ-methacryloxypropyltrimethoxysilane to the dispersion under stirring, the mass ratio of the added mass of the γ-methacryloxypropyltrimethoxysilane to the modified graphene in the dispersion is γ-methacryloxypropyltrimethoxysilane: modified graphene = 2:1; after the addition is completed, adjust the pH to 4 with hydrochloric acid (the mass percentage of the solute is 20%), and then heat in a water bath to 50±3°C in an argon protection atmosphere and stir for 3h, then separate the solid and liquid, wash the solid phase with ethanol 3 times, dry at 40°C for 20h, and after drying The solid phase is added to the mixed aqueous solution of acrylamide and acrylic acid, and the solid-liquid mass ratio of the dried solid phase to the mixed aqueous solution of acrylamide and acrylic acid is 1:80. After adding, stirring is carried out for 20 minutes, and then N, N-methylenebisacrylamide is added to the solution under stirring. After the addition is completed, stirring is continued for 20 minutes. Then, the mixed solution is placed in an argon protection atmosphere, heated to 60±3° C. in a water bath, and then an initiator is added. The added mass of the N, N-methylenebisacrylamide and the initiator is the same as that of the mixture. The mass ratio of the dried solid phase added to the mixed aqueous solution of acrylamide and acrylic acid is N,N-methylenebisacrylamide:initiator:dried solid phase=1.4:0.2:1; the initiator is ammonium persulfate; after the addition is completed, the mixture is kept warm and stirred at 60±3°C in an argon atmosphere for 2 hours, then the solid and liquid are separated, the solid phase is washed twice with ethanol, then washed twice with deionized water, and dried at 50°C for 10 hours, the dried solid phase is evenly mixed with zinc powder passed through a 1000-mesh sieve, and the mass ratio of the dried solid phase to the zinc powder is dried solid phase: zinc powder=1:3, to obtain the precipitant.

[0038] Example 3

[0039] A method for producing active zinc oxide by a wet process, comprising the steps of:

[0040] (1) Grinding zinc-containing furnace tailings (the main chemical composition analysis results are shown in Table 1) into powder, and soaking the powder in a sulfuric acid solution, wherein the mass ratio of the solute in the sulfuric acid solution is 30%, and the solid-liquid mass ratio of the powder soaked in the sulfuric acid solution is powder: sulfuric acid solution = 1:10; heating in a water bath to 55±5°C, keeping the temperature and stirring for 1h, and then air cooling to room temperature, solid-liquid separation, and obtaining a leachate;

[0041] (2) preparing a mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide; in the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide, the mass percentage of H2O2 is 20%, the mass percentage of dodecylbenzenesulfonic acid is 3%, and the solvent is water; stirring the leachate, and then adding the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide to the leachate under stirring to obtain a mixed solution, wherein the volume ratio of the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide added to the leachate is leachate:mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide=10:4; after the addition is completed, continuing to stir the mixed solution for 30 minutes to oxidize the ferrous ions to form ferric ions;

[0042] (3) preparing a precipitant; stirring the mixed solution, and then adding the precipitant to the mixed solution under stirring, wherein the mass ratio of the precipitant added to the mixed solution is mixed solution: precipitant = 10:2; heating the mixture to 50±5° C. in a water bath and stirring for 20 min, then performing solid-liquid separation to obtain a filtrate and a filter residue, soaking the filter residue in a dilute hydrochloric acid solution (5% by mass of the solute) and performing ultrasonic vibration for 10 min, performing a reactivation treatment on the precipitant, removing adsorbed lead and cadmium ions, then performing solid-liquid separation, washing the solid phase with deionized water until the washed solution is neutral, then soaking the solid phase in the filtrate again, heating the mixture to 50±5° C. in a water bath and stirring for 20 min, and performing solid-liquid separation after the insulation to obtain a zinc-containing liquid;

[0043] (4) adding sodium carbonate to the zinc-containing solution, wherein the mass ratio of sodium carbonate to the zinc-containing solution is zinc-containing solution: sodium carbonate = 100:12; heating in a water bath to 60±5° C. and stirring for 1 h to obtain basic zinc carbonate precipitate, separating the solid from the liquid, washing the solid phase with deionized water for 3 times, and then calcining and decomposing the precipitate at a calcination temperature of 800° C. for 1 h to generate the active zinc oxide;

[0044] The preparation method of the precipitant is as follows:

[0045] Step 1, prepare an aqueous solution of sodium hydroxide; in the aqueous solution of sodium hydroxide, the concentration of sodium hydroxide is 11g / 100mL, and the solvent is water; add graphene oxide to the aqueous solution of sodium hydroxide, stir for 30min, and then add carbon disulfide to the solution under stirring, the mass ratio of graphene oxide and carbon disulfide added to the aqueous solution of sodium hydroxide is graphene oxide: carbon disulfide: aqueous solution of sodium hydroxide = 4:7:100; after the addition is completed, stir for 20min, then heat in a water bath to 40±3°C and keep stirring for 5h, separate the solid and liquid after the insulation is completed, wash the solid phase with ethanol 3 times, then wash with deionized water 3 times, and dry at 40°C for 20h to obtain modified graphene;

[0046] Step 2, preparing an aqueous solution of ethanol; the volume percentage of ethanol in the aqueous solution of ethanol is 60%; preparing a mixed aqueous solution of acrylamide and acrylic acid; in the mixed aqueous solution of acrylamide and acrylic acid, the concentration of acrylamide is 4.4g / 100mL, the concentration of acrylic acid is 2.3g / 100mL, and the solvent is water; adding the modified graphene to the aqueous solution of ethanol, the solid-liquid mass ratio of the modified graphene added to the aqueous solution of ethanol is modified graphene: ethanol aqueous solution = 1:50; stirring and dispersing under ultrasonic environment for 30min to obtain dispersion, and then adding γ-methacryloxypropyltrimethoxysilane to the dispersion under stirring, the mass ratio of the added mass of γ-methacryloxypropyltrimethoxysilane to the modified graphene in the dispersion is γ-methacryloxypropyltrimethoxysilane: modified graphene = 2:1; after the addition is completed, the pH is adjusted to 4 with hydrochloric acid (the mass percentage of the solute is 20%), and then heated to 50±3°C in a water bath in an argon protective atmosphere and stirred for 3h, and then the solid-liquid separation is carried out, the solid phase is washed 3 times with ethanol, and dried at 40°C for 20h, and dried The solid phase after drying is added to the mixed aqueous solution of acrylamide and acrylic acid, and the solid-liquid mass ratio of the solid phase after drying to the mixed aqueous solution of acrylamide and acrylic acid is the solid phase after drying: the mixed aqueous solution of acrylamide and acrylic acid = 1:80. After adding, stir for 20 minutes, and then add N, N-methylenebisacrylamide to the solution under stirring. After the addition is completed, continue to stir for 20 minutes, and then place the mixed solution in an argon protection atmosphere, heat it in a water bath to 60 ± 3 ° C for insulation, and then add the initiator. The added mass of the N, N-methylenebisacrylamide and the initiator is the same as that of the initiator. The mass ratio of the dried solid phase added to the mixed aqueous solution of acrylamide and acrylic acid is N,N-methylenebisacrylamide:initiator:dried solid phase=1.4:0.3:1; the initiator is ammonium persulfate; after the addition is completed, the mixture is kept warm and stirred at 60±3°C in an argon atmosphere for 2 hours, then the solid and liquid are separated, the solid phase is washed twice with ethanol, then washed twice with deionized water, and dried at 50°C for 10 hours, the dried solid phase is evenly mixed with zinc powder passed through a 1000-mesh sieve, and the mass ratio of the dried solid phase to the zinc powder is dried solid phase: zinc powder=1:3, to obtain the precipitant.

[0047] Example 4

[0048] A method for producing active zinc oxide by a wet process, comprising the steps of:

[0049] (1) Grinding zinc-containing furnace tailings (the main chemical composition analysis results are shown in Table 1) into powder, and soaking the powder in a sulfuric acid solution, wherein the mass ratio of the solute in the sulfuric acid solution is 30%, and the solid-liquid mass ratio of the powder soaked in the sulfuric acid solution is powder: sulfuric acid solution = 1:10; heating in a water bath to 55±5°C, keeping the temperature and stirring for 1h, and then air cooling to room temperature, solid-liquid separation, and obtaining a leachate;

[0050] (2) preparing a mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide; in the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide, the mass percentage of H2O2 is 20%, the mass percentage of dodecylbenzenesulfonic acid is 3%, and the solvent is water; stirring the leachate, and then adding the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide to the leachate under stirring to obtain a mixed solution, wherein the volume ratio of the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide added to the leachate is leachate:mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide=10:4; after the addition is completed, continuing to stir the mixed solution for 30 minutes to oxidize the ferrous ions to form ferric ions;

[0051] (3) preparing a precipitant; stirring the mixed solution, and then adding the precipitant to the mixed solution under stirring, wherein the mass ratio of the precipitant added to the mixed solution is mixed solution: precipitant = 10:3; heating the mixture to 50±5° C. in a water bath and stirring for 20 min, then performing solid-liquid separation to obtain a filtrate and a filter residue, soaking the filter residue in a dilute hydrochloric acid solution (5% by mass of the solute) and performing ultrasonic vibration for 10 min, performing a reactivation treatment on the precipitant, removing adsorbed lead and cadmium ions, then performing solid-liquid separation, washing the solid phase with deionized water until the washed liquid is neutral, then soaking the solid phase in the filtrate again, heating the mixture to 50±5° C. in a water bath and stirring for 20 min, and performing solid-liquid separation after the insulation to obtain a zinc-containing liquid;

[0052] (4) adding sodium carbonate to the zinc-containing solution, wherein the mass ratio of sodium carbonate to the zinc-containing solution is zinc-containing solution: sodium carbonate = 100:14; heating in a water bath to 60±5° C. and stirring for 1 h to obtain basic zinc carbonate precipitate, separating the solid from the liquid, washing the solid phase with deionized water for 3 times, and then calcining and decomposing the precipitate at a calcination temperature of 800° C. for 1 h to generate the active zinc oxide;

[0053] The preparation method of the precipitant is as follows:

[0054] Step 1, prepare an aqueous solution of sodium hydroxide; in the aqueous solution of sodium hydroxide, the concentration of sodium hydroxide is 12g / 100mL, and the solvent is water; add graphene oxide to the aqueous solution of sodium hydroxide, stir for 30min, and then add carbon disulfide to the solution under stirring, the mass ratio of graphene oxide and carbon disulfide added to the aqueous solution of sodium hydroxide is graphene oxide: carbon disulfide: aqueous solution of sodium hydroxide = 4:7:100; after the addition is completed, stir for 20min, then heat in a water bath to 40±3°C and keep stirring for 5h, separate the solid and liquid after the insulation is completed, wash the solid phase with ethanol 3 times, then wash with deionized water 3 times, and dry at 40°C for 20h to obtain modified graphene;

[0055] Step 2, prepare an aqueous solution of ethanol; the volume percentage of ethanol in the aqueous solution of ethanol is 60%; prepare a mixed aqueous solution of acrylamide and acrylic acid; in the mixed aqueous solution of acrylamide and acrylic acid, the concentration of acrylamide is 4.6g / 100mL, the concentration of acrylic acid is 2.5g / 100mL, and the solvent is water; add the modified graphene to the aqueous solution of ethanol, the solid-liquid mass ratio of the modified graphene added to the aqueous solution of ethanol is modified graphene: ethanol aqueous solution = 1:50; stir and disperse for 30 minutes under an ultrasonic environment to obtain dispersion, and then adding γ-methacryloxypropyltrimethoxysilane to the dispersion under stirring, the mass ratio of the added mass of γ-methacryloxypropyltrimethoxysilane to the modified graphene in the dispersion is γ-methacryloxypropyltrimethoxysilane: modified graphene = 2:1; after the addition is completed, the pH is adjusted to 4 with hydrochloric acid (the mass percentage of the solute is 20%), and then heated to 50±3°C in a water bath in an argon protective atmosphere and stirred for 3h, and then the solid-liquid separation is carried out, the solid phase is washed 3 times with ethanol, and dried at 40°C for 20h, and dried The solid phase after drying is added to the mixed aqueous solution of acrylamide and acrylic acid, and the solid-liquid mass ratio of the solid phase after drying to the mixed aqueous solution of acrylamide and acrylic acid is the solid phase after drying: the mixed aqueous solution of acrylamide and acrylic acid = 1:80. After adding, stir for 20 minutes, and then add N, N-methylenebisacrylamide to the solution under stirring. After the addition is completed, continue to stir for 20 minutes, and then place the mixed solution in an argon protection atmosphere, heat it in a water bath to 60 ± 3 ° C for insulation, and then add the initiator. The added mass of the N, N-methylenebisacrylamide and the initiator is the same as that of the initiator. The mass ratio of the dried solid phase added to the mixed aqueous solution of acrylamide and acrylic acid is N,N-methylenebisacrylamide:initiator:dried solid phase=1.6:0.3:1; the initiator is ammonium persulfate; after the addition is completed, the mixture is kept warm and stirred at 60±3°C in an argon atmosphere for 2 hours, then the solid and liquid are separated, the solid phase is washed twice with ethanol, then washed twice with deionized water, and dried at 50°C for 10 hours, the dried solid phase is evenly mixed with zinc powder passed through a 1000-mesh sieve, and the mass ratio of the dried solid phase to the zinc powder is dried solid phase: zinc powder=1:3, to obtain the precipitant.

[0056] Comparative Example 1

[0057] A comparative method for producing active zinc oxide by a wet process comprises the following steps:

[0058] (1) Grinding zinc-containing furnace tailings (the main chemical composition analysis results are shown in Table 1) into powder, and soaking the powder in a sulfuric acid solution, wherein the mass ratio of the solute in the sulfuric acid solution is 30%, and the solid-liquid mass ratio of the powder soaked in the sulfuric acid solution is powder: sulfuric acid solution = 1:10; heating in a water bath to 55±5°C, keeping the temperature and stirring for 1h, and then air cooling to room temperature, solid-liquid separation, and obtaining a leachate;

[0059] (2) preparing a mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide; in the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide, the mass percentage of H2O2 is 20%, the mass percentage of dodecylbenzenesulfonic acid is 2%, and the solvent is water; stirring the leachate, and then adding the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide to the leachate under stirring to obtain a mixed solution, wherein the volume ratio of the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide added to the leachate is leachate: mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide = 10:3; after the addition is completed, continuing to stir the mixed solution for 30 minutes to oxidize the ferrous ions to form ferric ions;

[0060] (3) preparing a precipitant; stirring the mixed solution, and then adding the precipitant to the mixed solution under stirring, wherein the mass ratio of the precipitant added to the mixed solution is mixed solution: precipitant = 10:2; heating the mixture to 50±5° C. in a water bath and stirring for 20 min, then performing solid-liquid separation to obtain a filtrate and a filter residue, soaking the filter residue in a dilute hydrochloric acid solution (5% by mass of the solute) and performing ultrasonic vibration for 10 min, performing a reactivation treatment on the precipitant, removing adsorbed lead and cadmium ions, then performing solid-liquid separation, washing the solid phase with deionized water until the washed solution is neutral, then soaking the solid phase in the filtrate again, heating the mixture to 50±5° C. in a water bath and stirring for 20 min, and performing solid-liquid separation after the insulation to obtain a zinc-containing liquid;

[0061] (4) adding sodium carbonate to the zinc-containing solution, wherein the mass ratio of sodium carbonate to the zinc-containing solution is zinc-containing solution: sodium carbonate = 100:12; heating in a water bath to 60±5° C. and stirring for 1 h to obtain basic zinc carbonate precipitate, separating the solid from the liquid, washing the solid phase with deionized water for 3 times, and then calcining and decomposing the precipitate at a calcination temperature of 800° C. for 1 h to generate the active zinc oxide;

[0062] The preparation method of the precipitant is as follows: preparing an aqueous solution of ethanol; the volume percentage of ethanol in the aqueous solution of ethanol is 60%; preparing a mixed aqueous solution of acrylamide and acrylic acid; in the mixed aqueous solution of acrylamide and acrylic acid, the concentration of acrylamide is 4.4g / 100mL, the concentration of acrylic acid is 2g / 100mL, and the solvent is water; adding graphene oxide to the aqueous solution of ethanol, the solid-liquid mass ratio of the graphene oxide added to the aqueous solution of ethanol is graphene oxide: ethanol aqueous solution = 1:50; stirring and dispersing under an ultrasonic environment for 30min n obtain a dispersion, and then add γ-methacryloxypropyltrimethoxysilane to the dispersion under stirring, the mass ratio of the added mass of the γ-methacryloxypropyltrimethoxysilane to the mass ratio of the graphene oxide in the dispersion is γ-methacryloxypropyltrimethoxysilane:graphene oxide=2:1; after the addition is completed, adjust the pH to 4 with hydrochloric acid (the mass percentage of the solute is 20%), and then heat to 50±3° C. in a water bath in an argon protection atmosphere and keep stirring for 3 hours, then separate the solid and liquid, wash the solid phase with ethanol 3 times, dry it at 40° C. for 20 hours, and dry it The dried solid phase is added to the mixed aqueous solution of acrylamide and acrylic acid, and the solid-liquid mass ratio of the dried solid phase to the mixed aqueous solution of acrylamide and acrylic acid is 1:80. After adding, stirring is carried out for 20 minutes, and then N, N-methylenebisacrylamide is added to the solution under stirring. After the addition is completed, stirring is continued for 20 minutes. Then, the mixed solution is placed in an argon protection atmosphere, heated to 60±3° C. in a water bath for insulation, and then an initiator is added. The added mass of the N, N-methylenebisacrylamide and the initiator is the same as that of the acrylic acid. The mass ratio of the dried solid phase added to the mixed aqueous solution of olefin amide and acrylic acid is N,N-methylenebisacrylamide:initiator:dried solid phase=1.4:0.2:1; the initiator is ammonium persulfate; after the addition is completed, the mixture is kept warm and stirred at 60±3°C in an argon atmosphere for 2h, then the solid-liquid is separated, the solid phase is washed twice with ethanol, then washed twice with deionized water, and dried at 50°C for 10h, the dried solid phase is evenly mixed with zinc powder passed through a 1000-mesh sieve, and the mass ratio of the dried solid phase to the zinc powder is dried solid phase: zinc powder=1:3, to obtain the precipitant described in this comparative example.

[0063] Comparative Example 2

[0064] A comparative method for producing active zinc oxide by a wet process comprises the following steps:

[0065] (1) Grinding zinc-containing furnace tailings (the main chemical composition analysis results are shown in Table 1) into powder, and soaking the powder in a sulfuric acid solution, wherein the mass ratio of the solute in the sulfuric acid solution is 30%, and the solid-liquid mass ratio of the powder soaked in the sulfuric acid solution is powder: sulfuric acid solution = 1:10; heating in a water bath to 55±5°C, keeping the temperature and stirring for 1h, and then air cooling to room temperature, solid-liquid separation, and obtaining a leachate;

[0066] (2) preparing a mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide; in the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide, the mass percentage of H2O2 is 20%, the mass percentage of dodecylbenzenesulfonic acid is 2%, and the solvent is water; stirring the leachate, and then adding the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide to the leachate under stirring to obtain a mixed solution, wherein the volume ratio of the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide added to the leachate is leachate: mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide = 10:3; after the addition is completed, continuing to stir the mixed solution for 30 minutes to oxidize the ferrous ions to form ferric ions;

[0067] (3) preparing a precipitant; stirring the mixed solution, and then adding the precipitant to the mixed solution under stirring, wherein the mass ratio of the precipitant added to the mixed solution is mixed solution: precipitant = 10:2; heating the mixture to 50±5° C. in a water bath and stirring for 20 min, then performing solid-liquid separation to obtain a filtrate and a filter residue, soaking the filter residue in a dilute hydrochloric acid solution (5% by mass of the solute) and performing ultrasonic vibration for 10 min, performing a reactivation treatment on the precipitant, removing adsorbed lead and cadmium ions, then performing solid-liquid separation, washing the solid phase with deionized water until the washed solution is neutral, then soaking the solid phase in the filtrate again, heating the mixture to 50±5° C. in a water bath and stirring for 20 min, and performing solid-liquid separation after the insulation to obtain a zinc-containing liquid;

[0068] (4) adding sodium carbonate to the zinc-containing solution, wherein the mass ratio of sodium carbonate to the zinc-containing solution is zinc-containing solution: sodium carbonate = 100:12; heating in a water bath to 60±5° C. and stirring for 1 h to obtain basic zinc carbonate precipitate, separating the solid from the liquid, washing the solid phase with deionized water for 3 times, and then calcining and decomposing the precipitate at a calcination temperature of 800° C. for 1 h to generate the active zinc oxide;

[0069] The preparation method of the precipitant is as follows:

[0070] Step 1, prepare an aqueous solution of sodium hydroxide; in the aqueous solution of sodium hydroxide, the concentration of sodium hydroxide is 11g / 100mL, and the solvent is water; add graphene oxide to the aqueous solution of sodium hydroxide, stir for 30min, and then add carbon disulfide to the solution under stirring, the mass ratio of graphene oxide and carbon disulfide added to the aqueous solution of sodium hydroxide is graphene oxide: carbon disulfide: aqueous solution of sodium hydroxide = 3:6:100; after the addition is completed, stir for 20min, then heat in a water bath to 40±3°C and keep stirring for 5h, separate the solid and liquid after the insulation is completed, wash the solid phase with ethanol 3 times, then wash with deionized water 3 times, and dry at 40°C for 20h to obtain modified graphene;

[0071] Step 2, preparing an aqueous solution of ethanol; the volume percentage of ethanol in the aqueous solution of ethanol is 60%; adding the modified graphene to the aqueous solution of ethanol, the solid-liquid mass ratio of the modified graphene added to the aqueous solution of ethanol is modified graphene: ethanol aqueous solution = 1:50; stirring and dispersing for 30 minutes under an ultrasonic environment to obtain a dispersion, and then adding γ-methacryloxypropyltrimethoxysilane to the dispersion under stirring, the mass of the γ-methacryloxypropyltrimethoxysilane added is equal to the mass of the dispersion The mass ratio of modified graphene is γ-methacryloxypropyltrimethoxysilane: modified graphene = 2:1; after the addition is completed, the pH is adjusted to 4 with hydrochloric acid (the mass percentage of the solute is 20%), and then heated to 50±3°C in a water bath in an argon protective atmosphere and stirred for 3 hours, then the solid-liquid separation is carried out, the solid phase is washed 3 times with ethanol, and dried at 40°C for 20 hours. The dried solid phase is evenly mixed with zinc powder passed through a 1000 mesh sieve, and the mass ratio of the dried solid phase to the zinc powder is the dried solid phase: zinc powder = 1:3, and the precipitant described in this comparative example is obtained.

[0072] Example 5

[0073] The purity of zinc oxide in the products prepared by the methods described in the examples and comparative examples was tested, and the results are shown in Table 2.

[0074] As can be seen from Table 2, the product zinc oxide obtained by the method of the present invention has a high purity and meets the requirements for high-purity active zinc oxide. The present invention introduces a new precipitant on the basis of the traditional zinc powder reduction and impurity removal process, which further reduces the content of impurity elements in the product. Although the traditional zinc powder replacement process can effectively remove heavy metal ions such as iron, when the concentration of heavy metal ions is low, the effect of zinc replacement is not good. Therefore, it is difficult to further reduce the content of impurity elements in the product when the impurity ion content is low. The present invention introduces a precipitant, utilizes a large number of dithiocarboxyl groups formed on the surface of graphene oxide, and a large number of C=O, C-O, and carboxylic acid functional groups in the macromolecular structure of polyacrylamide, so that the ion Pb2+ 、Cd 2+ , and these functional groups undergo complexation and ion exchange, and can effectively remove Pb at low concentrations. 2+ 、Cd 2+ The selective adsorption of ions is more obvious, while the effect on zinc ions is smaller. This may be related to the adsorption competition caused by the different adsorption difficulties of different ions.

[0075] Table 1

[0076]

[0077] Table 2

[0078] Element Purity of zinc oxide (wt%) Example 1 99.86 Example 2 99.95 Example 3 99.92 Example 4 99.94 Comparative Example 1 99.13 Comparative Example 2 99.08

[0079] The technical solution provided by the present invention is introduced in detail above. For those skilled in the art, according to the concept of the embodiments of the present invention, there may be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A method for producing active zinc oxide by a wet process, characterized in that the steps include: (1) Grind the zinc-containing furnace tailings into powder, soak the powder in a sulfuric acid solution, heat it in a water bath to 55±5°C, keep it warm and stir it for more than 1 hour, then air cool it to room temperature, separate the solid and liquid, and obtain a leachate; (2) preparing a mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide; stirring the leachate, and then adding the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide to the leachate under stirring to obtain a mixed solution, and continuing to stir the mixed solution for more than 30 minutes after the addition is completed to oxidize the ferrous ions to form ferric ions; (3) preparing a precipitant; stirring the mixed solution, then adding the precipitant to the mixed solution under stirring, heating the mixed solution to 50±5° C. in a water bath and stirring for more than 20 minutes, then separating the solid and the liquid to obtain a filtrate and a filter residue, soaking the filter residue in a dilute hydrochloric acid solution and ultrasonically vibrating for more than 10 minutes, then separating the solid and the liquid, washing the solid phase with deionized water until the washed solution is neutral, then soaking the solid phase in the filtrate again, heating the mixed solution to 50±5° C. in a water bath and stirring for more than 20 minutes, and then separating the solid and the liquid after the insulation to obtain a zinc-containing liquid; (4) adding sodium carbonate to the zinc-containing solution, heating in a water bath to 60±5° C. and stirring for more than 1 hour to obtain basic zinc carbonate precipitate, separating the solid from the liquid, washing the solid phase with deionized water for more than 3 times, and then calcining and decomposing to generate the active zinc oxide; The preparation method of the precipitant is as follows: Step 1, preparing an aqueous solution of sodium hydroxide; adding graphene oxide to the aqueous solution of sodium hydroxide, stirring for more than 30 minutes, then adding carbon disulfide to the solution under stirring, stirring for more than 20 minutes after the addition is completed, and then heating in a water bath to 40±3°C and stirring for more than 5 hours, separating the solid and the liquid after the insulation is completed, washing the solid phase with ethanol for more than 3 times, and then washing with deionized water for more than 3 times, and drying at 40°C for more than 20 hours to obtain modified graphene; Step 2, preparing an aqueous solution of ethanol; preparing a mixed aqueous solution of acrylamide and acrylic acid; adding the modified graphene to the aqueous solution of ethanol, stirring and dispersing for more than 30 minutes under an ultrasonic environment to obtain a dispersion, and then adding γ-methacryloxypropyltrimethoxysilane to the dispersion under stirring. After the addition is completed, the pH is adjusted to 4 with hydrochloric acid, and then heated to 50±3°C in a water bath in an argon protection atmosphere and stirred for more than 3 hours, and then the solid-liquid separation is performed, and the solid phase is washed with ethanol for more than 3 times, and dried at 40°C for more than 20 hours. After drying, the solid phase is added to the mixed aqueous solution of acrylamide and acrylic acid, and stirred for 20 minutes after adding. min or more, then add N,N-methylenebisacrylamide to the solution under stirring, continue stirring for more than 20 min after the addition is completed, then place the mixed solution in an argon protection atmosphere, heat to 60±3° C. in a water bath, then add an initiator, and after the addition is completed, keep stirring at 60±3° C. in an argon atmosphere for more than 2 h, then separate the solid and liquid, wash the solid phase with ethanol for more than 2 times, then wash it with deionized water for more than 2 times, dry it at 50° C. for more than 10 h, mix the dried solid phase with zinc powder through a 1000-mesh sieve, and mix the dried solid phase with zinc powder in a mass ratio of dried solid phase to zinc powder of 1:3 to obtain the precipitant.

2. The method for producing active zinc oxide by a wet process according to claim 1, characterized in that: In the step (1), the mass percentage of the solute in the sulfuric acid solution is 30%, and the solid-liquid mass ratio of the powder immersed in the sulfuric acid solution is powder: sulfuric acid solution = 1:

10.

3. The method for producing active zinc oxide by a wet process according to claim 1, characterized in that: In the step (2), in the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide, the mass percentage of H2O2 is 20%, the mass percentage of dodecylbenzenesulfonic acid is 2% to 3%, and the solvent is water; the volume ratio of the mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide added to the leachate is leachate:mixed solution of dodecylbenzenesulfonic acid and hydrogen peroxide=10:3 to 4.

4. The method for producing active zinc oxide by a wet process according to claim 1, characterized in that: In the step (3), the mass ratio of the precipitant added to the mixed solution is mixed solution:precipitant=10:1-3.

5. The method for producing active zinc oxide by a wet process according to claim 1, characterized in that: In the step (4), the mass ratio of sodium carbonate added to the zinc-containing liquid is zinc-containing liquid: sodium carbonate = 100:10-14; the calcination temperature is 800° C., and the calcination time is 1 hour.

6. The method for producing active zinc oxide by a wet process according to claim 1, characterized in that: In the step 1, the concentration of sodium hydroxide in the aqueous solution of sodium hydroxide is 10-12 g / 100 mL, and the solvent is water; the mass ratio of the added mass of graphene oxide and carbon disulfide to the aqueous solution of sodium hydroxide is graphene oxide: carbon disulfide: aqueous solution of sodium hydroxide = 3-4:6-7:

100.

7. The method for producing active zinc oxide by a wet process according to claim 1, characterized in that: In the step 2, the volume percentage of ethanol in the ethanol aqueous solution is 60%; in the mixed aqueous solution of acrylamide and acrylic acid, the concentration of acrylamide is 4.2-4.6 g / 100 mL, the concentration of acrylic acid is 1.7-2.5 g / 100 mL, and the solvent is water; the modified graphene is added to the ethanol aqueous solution at a solid-liquid mass ratio of modified graphene: ethanol aqueous solution = 1:50; the mass ratio of the added mass of γ-methacryloxypropyltrimethoxysilane to the mass of the modified graphene in the dispersion is γ-methacryloxypropyltrimethoxysilane. The mass ratio of methoxysilane to modified graphene is 2:1; the mass percentage of the solute in the hydrochloric acid is 20%; the solid-liquid mass ratio of the dried solid phase added to the mixed aqueous solution of acrylamide and acrylic acid is the dried solid phase: the mixed aqueous solution of acrylamide and acrylic acid is 1:80; the mass ratio of the added N,N-methylenebisacrylamide and initiator to the dried solid phase added to the mixed aqueous solution of acrylamide and acrylic acid is N,N-methylenebisacrylamide: initiator: dried solid phase is 1.2-1.6:0.2-0.3:1; the initiator is ammonium persulfate.

Citation Information

Patent Citations

  • Preparation method and application of magnetic graphene oxide adsorbent material

    CN105289515A

  • Preparation method of high-purity zinc oxide

    CN106853982A

  • Method for producing activated zinc oxide by wet process

    CN111747442A

  • Prepn. of znso4 and active zno from zinc ore by entire wet-process

    CN86108798A