Preparation method of ferrous sulfate
Ferrous sulfate was prepared in the electrolytic cell by electrochemical reduction method, and impurities were separated by proton permeable membrane, which solved the problems of impurities introduction and economic cost in the existing methods, and achieved high purity and low-cost preparation of ferrous sulfate.
Patent Information
- Application Number
- CN202411124150.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-08
AI Technical Summary
The existing ferrous sulfate preparation methods include the introduction of impurities, high economic costs, and increased equipment investment.
The electrochemical reduction method is used to place the iron sulfate solution in the cathode region of the electrolytic cell for electrochemical reduction, and the impurities are separated by proton permeation membrane. The anode undergoes a water oxidation reaction to generate oxygen, with a voltage of 1.5 to 1.7V and a time of 2 to 7 hours. , and then concentrated, crystallized, filtered and dried.
The preparation of high-purity ferrous sulfate is realized, which reduces production costs, avoids the introduction of impurities and equipment increase, and improves production efficiency.
Smart Images

Figure CN118908293A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of inorganic chemical industry, and particularly relates to a method for preparing ferrous sulfate. Background Art
[0002] Iron in a high valence state (trivalent) is conducive to removing metal ion impurities to obtain high-purity iron sulfate. Compared with ferric sulfate, ferrous sulfate has greater market demand and commercial value, and is widely used in the fields of new energy batteries, medicine, and magnetic materials.
[0003] At present, the method for preparing ferrous sulfate is mainly to carry out chemical reduction with ferrous sulfate as raw material, and the specific method is to add a reducing substance (such as sodium sulfide or ascorbic acid) to a ferrous sulfate solution, obtain a ferrous sulfate solution through an oxidation-reduction reaction, and then obtain ferrous sulfate crystals through recrystallization. The existing method has three significant defects: 1. Introducing new impurities, including impurities contained in the reducing substance itself and impurities that cannot be completely separated and brought in after the reducing substance is oxidized. 2. The economic cost is high, and the price of this type of chemical reducing substance itself is also relatively expensive, especially the reductant with higher purity, which increases the production cost and reduces the profit margin of the final product ferrous sulfate. 3. The separation of the oxide generated after the reducing agent completes the chemical reduction process requires the addition of a new chemical unit, which increases equipment investment and operating costs.
[0004] How to efficiently prepare ferrous sulfate with higher purity is a technical problem that urgently needs to be solved. Summary of the invention
[0005] In view of this, the present invention provides a method for preparing ferrous sulfate. The preparation method provided by the present invention adopts a simple device and is easy to operate. The prepared product has high purity and low production cost.
[0006] In order to solve the above technical problems, the present invention provides a method for preparing ferrous sulfate, comprising the following steps:
[0007] Placing the ferric sulfate solution in the cathode region of the electrolytic cell for electrochemical reduction to obtain ferrous ferrite;
[0008] The electrolytic cell comprises a proton permeable membrane arranged in the center of the electrolytic cell; the voltage of the electrochemical reduction is 1.5-1.7V.
[0009] Preferably, the electrochemical reduction time is 2 to 7 hours.
[0010] Preferably, the proton permeable membrane comprises a nafionN117 proton permeable membrane.
[0011] Preferably, the electrolytic cell further comprises an anode disposed on one side of the proton permeable membrane, a cathode disposed on the other side of the proton permeable membrane, and a power source connecting the anode and the cathode;
[0012] The electrolyte on the anode side is a sulfuric acid solution.
[0013] Preferably, the anode includes a substrate and a catalyst, and the catalyst is loaded on the surface of the titanium mesh or the surface of the proton permeable membrane facing the anode pool; when the catalyst is loaded on the surface of the proton permeable membrane facing the anode pool, the anode needs to be in direct contact with the proton permeable membrane.
[0014] Preferably, the substrate comprises a titanium mesh;
[0015] The catalyst comprises iridium oxide or ruthenium oxide;
[0016] The catalyst loading is 0.4-0.6 mg / cm 2 .
[0017] Preferably, the cathode material includes graphite or iron.
[0018] Preferably, the molar concentration of the ferric sulfate solution is 1.5 to 3.5 mol / L.
[0019] Preferably, the molar concentration of the sulfuric acid solution is consistent with the molar concentration of the ferric sulfate solution.
[0020] Preferably, after the electrochemical reduction, the process further comprises: sequentially concentrating, crystallizing, filtering and drying the system after the electrochemical reduction to obtain the ferrous sulfate.
[0021] The present invention provides a method for preparing ferrous sulfate, comprising the following steps: placing a ferrous sulfate solution in the cathode region of an electrolytic cell for electrochemical reduction to obtain ferrous ferrate; the electrolytic cell comprises a proton permeable membrane placed in the center of the electrolytic cell; the voltage of the electrochemical reduction is 1.5 to 1.7 V. In the electrochemical reduction process of the present invention, water oxidation reaction mainly occurs at the anode, and the generated oxygen diffuses into the air; the proton permeable membrane separates the cathode region and the anode region and only transmits protons to avoid excessive impurities generated in the cathode region. The device used in the preparation method provided by the present invention is simple and easy to operate, and the impurities generated during the preparation process are less, which improves the purity of ferrous sulfate. The preparation method provided by the present invention has a lower production cost for preparing ferrous sulfate. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Schematic diagram of the principle of electrochemical reduction reaction of ferric sulfate solution in an electrolytic cell. DETAILED DESCRIPTION
[0023] The present invention provides a method for preparing ferrous sulfate, comprising the following steps:
[0024] The ferric sulfate solution is placed in the cathode region of the electrolytic cell for electrochemical reduction to obtain ferrous ferrite.
[0025] In the present invention, the molar concentration of the ferric sulfate solution is preferably 1.5 to 3.5 mol / L, more preferably 2.5 to 3 mol / L.
[0026] In the present invention, the electrolytic cell comprises a proton permeable membrane placed in the center of the electrolytic cell. In the present invention, the proton permeable membrane preferably comprises a nafion N117 proton permeable membrane, and the nafion N117 proton permeable membrane is preferably purchased from DuPont.
[0027] In the present invention, the electrolytic cell preferably further comprises an anode disposed on one side of the proton permeable membrane, a cathode disposed on the other side of the proton permeable membrane, and a power source connecting the anode and the cathode. In the present invention, the anode preferably comprises a substrate and a catalyst, and the catalyst is preferably loaded on the surface of the titanium mesh or the surface of the proton permeable membrane facing the anode pool; when the catalyst is loaded on the surface of the proton permeable membrane facing the anode pool, the anode needs to be in direct contact with the proton permeable membrane. In the present invention, the substrate is preferably a titanium mesh; the catalyst preferably comprises iridium oxide or ruthenium oxide, more preferably iridium oxide; the loading amount of the catalyst is preferably 0.4-0.6 mg / cm 2 , more preferably 0.5 mg / cm 2 In the present invention, the electrolyte on the anode side is preferably a sulfuric acid solution. In the present invention, the molar concentration of the sulfuric acid solution is preferably consistent with the molar concentration of the ferric sulfate solution.
[0028] In the present invention, the cathode material preferably includes graphite or iron, more preferably iron; in the present invention, the cathode is preferably mesh-shaped or plate-shaped, more preferably mesh-shaped. In the present invention, the cathode reaction cell is preferably a flow reaction cell.
[0029] In the present invention, the electrolytic cell is preferably a flow electrolytic cell.
[0030] In the present invention, the voltage of the electrochemical reduction is 1.5 to 1.7 V, preferably 1.6 V; the time of the electrochemical reduction is preferably 2 to 7 hours, more preferably 4 to 6 hours.
[0031] In the present invention, Figure 1This is a schematic diagram of the principle of electrochemical reduction reaction in an electrolytic cell. Water oxidation reaction occurs at the anode to generate oxygen and provide electrons for the cathode reduction reaction. The proton permeable membrane can only pass protons but not other ions. The product protons penetrate into the solution through the proton permeable membrane and form an electric current. The product oxygen cannot pass through the proton permeable membrane and will not enter the solution to participate in the reaction, but will diffuse and be discharged. The trivalent iron ions are reduced to divalent at the cathode. The two electrodes are connected with a wire and a certain voltage is applied, and the electrochemical reduction reaction can proceed quickly. Making the cathode into a flow reaction cell can more efficiently implement the reduction reaction and separate the reduction products.
[0032] In the present invention, a large amount of oxygen is produced at the anode during the electrolysis (electrochemical reduction reaction); the color of the cathode gradually becomes lighter to light green, and the electrolysis current gradually decreases to a stable state. At this time, the indicator is used to detect the absence of trivalent iron ions, and the electrolysis reaches the end point. In the present invention, the indicator is preferably potassium thiocyanate.
[0033] In the present invention, the anode reaction equation is shown in (1), the cathode reaction equation is shown in (2), and the overall electrode reaction equation of the electrochemical reduction reaction is shown in (3):
[0034] Anode 2H 2 O→4H + +4e - +O 2 (1)
[0035] Cathode Fe 3+ +e - →Fe 2+ (2)
[0036] Total reaction 2H 2 O+4Fe 3+ →4Fe 2+ +4H + +O 2 (3).
[0037] In the present invention, the electrochemical reduction reaction equation is as shown in formula a:
[0038] 2H 2 O+2Fe 2 (SO 4 ) 3 →4FeSO 4 +2H 2 SO 4 +O 2 Formula a.
[0039] In the present invention, after the electrochemical reduction, it is preferred that the electrochemical reduction system is concentrated, crystallized, filtered, and dried in sequence to obtain the ferrous sulfate. The present invention preferably uses evaporation for concentration; the evaporation temperature is preferably 90-100°C, more preferably 95-98°C; the evaporation time is preferably 30-50min, more preferably 40-45min. In the present invention, the crystallization is preferably cooling crystallization. The present invention has no special requirements for the cooling crystallization, as long as the ferrous sulfate can be crystallized. The present invention has no special requirements for the filtration, and the conventional methods in the art can be used. The present invention preferably washes the solid obtained by filtration; the washing solvent is preferably water. In the present invention, the drying temperature is preferably 55-75°C, more preferably 60-70°C; the drying time is preferably 1-2h, more preferably 1.5-1.8h.
[0040] In the present invention, the ferrous sulfate is preferably ferrous sulfate heptahydrate.
[0041] The preparation method provided by the present invention does not introduce new impurities, and the byproduct generated at the cathode during the reaction is only sulfuric acid, without any new impurities, and does not require further impurity removal and separation, so that there is no need to add a new impurity removal chemical unit, and it is directly used for the next step of recrystallization to obtain high-purity ferrous sulfate. The anode byproduct oxygen can be used to prepare ozone for removing reducing impurities. The energy required for the preparation method provided by the present invention is electrical energy, and the working environment adaptability is strong. The preparation method provided by the present invention is easy to scale up experiments, and mass production is truly realized. The preparation method provided by the present invention realizes green, efficient, and low-cost reduction of ferrous sulfate to prepare high-purity ferrous sulfate.
[0042] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0043] Example 1
[0044] The proton permeable membrane used in the electrolytic cell of the embodiment is a Nafion N117 proton permeable membrane purchased from DuPont; a proton permeable membrane (0.5 mg / cm 2 The anode on one side of the iridium oxide catalyst is a titanium mesh, which is directly in contact with the proton permeable membrane, and the cathode on the other side of the proton permeable membrane is an iron mesh; the flow rate of the peristaltic pump in the flow electrolytic cell is 80 mL / min, so as to realize the circulation of the anode pool and the cathode pool;
[0045] 500 mL of 3 mol / L sulfuric acid solution was placed in the anode region, and 500 mL of 3 mol / L ferric sulfate solution was placed in the cathode region; electrochemical reduction was performed at a voltage of 1.6 V for 7 h (the cathode electrolyte was light green, and there was no color change after potassium thiocyanate indicator was dropped into the cathode electrolyte, indicating that the reaction reached the end point), the system after electrochemical reduction was evaporated and concentrated at 100° C. for 30 min, then cooled and crystallized, the system after crystallization was filtered, the filtered solid was washed with water, and then dried at 75° C. for 1 h to obtain 700.56 g of ferrous sulfate heptahydrate.
[0046] Example 2
[0047] The electrochemical reduction reaction was carried out using the electrolytic cell of Example 1, except that the flow rate of the peristaltic pump was 50 mL / min;
[0048] 300 mL of 3 mol / L sulfuric acid solution was placed in the anode region, and 300 mL of 3 mol / L ferric sulfate solution was placed in the cathode region; electrochemical reduction was performed at a voltage of 1.6 V for 4 h (the cathode electrolyte was light green, and there was no color change after the indicator was dropped into the cathode electrolyte, indicating that the reaction reached the end point), the system after electrochemical reduction was evaporated and concentrated at 100° C. for 1 h, and then cooled and crystallized, the system after crystallization was filtered, the filtered solid was washed with water, and then dried at 75° C. for 1 h to obtain 405.03 g of ferrous sulfate heptahydrate.
[0049] Example 3
[0050] The electrochemical reduction reaction is carried out using the electrolytic cell of Example 1;
[0051] 300 mL of 1.5 mol / L sulfuric acid solution was placed in the anode region, and 300 mL of 1.5 mol / L ferric sulfate solution was placed in the cathode region; electrochemical reduction was performed at a voltage of 1.6 V for 3 h (the cathode electrolyte was light green, and there was no color change after the cathode electrolyte was dropped into the indicator, indicating that the reaction reached the end point), the system after electrochemical reduction was evaporated and concentrated at 95° C. for 1 h, and then cooled and crystallized, the system after crystallization was filtered, the filtered solid was washed with water, and then dried at 75° C. for 1 h to obtain 205.9 g of ferrous sulfate heptahydrate.
[0052] Example 4
[0053] The electrochemical reduction reaction is carried out using the electrolytic cell of Example 1;
[0054] 500 mL of a sulfuric acid solution with a molar concentration of 1.15 mol / L was placed in the anode area, and 500 mL of a ferric sulfate solution with a molar concentration of 1.15 mol / L was placed in the cathode area; electrochemical reduction was carried out at a voltage of 1.6 V for 3 h (the cathode electrolyte was light green, and there was no color change after the cathode electrolyte was dropped into the indicator, indicating that the reaction reached the end point), the system after electrochemical reduction was evaporated and concentrated at 95° C. for 40 min, and then cooled and crystallized, the system after crystallization was filtered, the filtered solid was washed with water and dried at 70° C. for 1 h, and 256.7 g of ferrous sulfate heptahydrate was obtained.
[0055] Example 5
[0056] The electrochemical reduction reaction is carried out using the electrolytic cell of Example 1;
[0057] 500 mL of a sulfuric acid solution with a molar concentration of 1.15 mol / L was placed in the anode region, and 500 mL of a ferric sulfate solution with a molar concentration of 1.15 mol / L was placed in the cathode region; electrochemical reduction was performed at a voltage of 1.6 V for 3 h (the cathode electrolyte was light green, and there was no color change after the cathode electrolyte was dropped into the indicator, indicating that the reaction reached the end point), the system after electrochemical reduction was evaporated and concentrated at 100° C. for 1 h, and then cooled and crystallized, the system after crystallization was filtered, the filtered solid was washed with water, and then dried at 75° C. for 1 h to obtain 259.3 g of ferrous sulfate heptahydrate.
[0058] Example 6
[0059] The electrochemical reduction reaction is carried out using the electrolytic cell of Example 1;
[0060] 300 mL of sulfuric acid solution with a molar concentration of 1.5 mol / L was placed in the anode area, and 300 mL of ferric sulfate solution with a molar concentration of 1.5 mol / L was placed in the cathode area; electrochemical reduction was carried out at a voltage of 1.6 V for 3 hours (the cathode electrolyte was light green, and there was no color change after the cathode electrolyte was dropped into the indicator, indicating that the reaction reached the end point), the system after electrochemical reduction was evaporated and concentrated at 100° C. for 1 hour, and then cooled and crystallized, the system after crystallization was filtered, the filtered solid was washed with water and dried at 75° C. for 1 hour, and 210 g of ferrous sulfate heptahydrate was obtained.
[0061] The purity of the ferrous sulfate heptahydrate prepared in Examples 1 to 6 was detected by inductively coupled plasma mass spectrometry (ICP-MS), and the results are listed in Table 1; the yield results of the ferrous sulfate heptahydrate prepared in Examples 1 to 6 are listed in Table 1.
[0062] Table 1 Purity and yield of ferrous sulfate heptahydrate prepared in Examples 1 to 6
[0063]
[0064]
[0065] It can be seen from Table 1 that the ferrous sulfate heptahydrate prepared according to the preparation method provided by the present invention has higher purity and higher yield.
[0066] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing ferrous sulfate, It is characterized in that The following steps are involved: Placing the ferric sulfate solution in the cathode region of the electrolytic cell for electrochemical reduction to obtain ferrous ferrite; The electrolytic cell comprises a proton permeable membrane arranged in the center of the electrolytic cell; the voltage of the electrochemical reduction is 1.5-1.7V.
2. The preparation method according to claim 1, It is characterized in that The electrochemical reduction time is 2 to 7 hours.
3. The preparation method according to claim 1, It is characterized in that The proton permeable membrane comprises a nafion N117 proton permeable membrane.
4. The preparation method according to claim 1, It is characterized in that The electrolytic cell also includes an anode disposed on one side of the proton permeable membrane, a cathode disposed on the other side of the proton permeable membrane, and a power source connected to the anode and the cathode; The electrolyte on the anode side is a sulfuric acid solution.
5. The preparation method according to claim 4, It is characterized in that The anode includes a substrate and a catalyst, and the catalyst is loaded on the surface of the titanium mesh or the surface of the proton permeable membrane facing the anode pool; when the catalyst is loaded on the surface of the proton permeable membrane facing the anode pool, the anode needs to be in direct contact with the proton permeable membrane.
6. The preparation method according to claim 5, It is characterized in that The substrate includes a titanium mesh; The catalyst comprises iridium oxide or ruthenium oxide; The catalyst loading is 0.4-0.6 mg / cm 2 .
7. The preparation method according to claim 4, It is characterized in that The cathode material includes graphite or iron.
8. The preparation method according to any one of claims 4 to 7, It is characterized in that The molar concentration of the ferric sulfate solution is 1.5-3.5 mol / L.
9. The preparation method according to any one of claims 4 to 7, It is characterized in that The molar concentration of the sulfuric acid solution is consistent with the molar concentration of the ferric sulfate solution.
10. The preparation method according to claim 1, It is characterized in that After the electrochemical reduction, the method further comprises: sequentially concentrating, crystallizing, filtering and drying the system after the electrochemical reduction to obtain the ferrous sulfate.