Corrosion inhibitor for cooling water system of marine diesel engine as well as preparation method and application of corrosion inhibitor
By using specific corrosion inhibitors in marine diesel engine cooling water systems to form a protective film, the electrochemical, chemical and cavitation problems of metal components under high temperature and high pressure are solved, and effective corrosion inhibition and scale inhibition effects are achieved, which extends the The service life of the cooling water system.
Patent Information
- Application Number
- CN202411343190.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The cooling water system of marine diesel engines is prone to a variety of corrosion under high temperature and high pressure conditions, including electrochemical corrosion, chemical corrosion and cavitation, which leads to accelerate corrosion of metal components, and the existing technology has not effectively solved the problem of high temperature and high pressure corrosion.
It is made of methyl diethanolamine, ethanolamine, cetylamine, benzotriazole, polyaspartic acid, sodium polyacrylate, aliphatic dibasic acid, neodecanoic acid, borax, alkyl alcohol amide, Corrosion inhibitor composed of propylene oxide condensate, ethylene oxide condensate, phosphonocarboxylic acid copolymer and purified water is prepared through neutralization reaction to form an organic film on the metal surface. , prevents the diffusion of water and dissolved oxygen, inhibits electrochemical and chemical corrosion, and has the ability to resist scale.
Effectively inhibit the electrochemical corrosion of various metals in high-temperature cooling water, prevent chemical corrosion caused by chloride ions and silicate ions, stabilize under high-pressure and high-temperature conditions, and is not easy to decompose, forming a protective film, and prevent cavitation caused by bubble bursting. It also has microbial inhibitory function to extend the service life of the cooling water system.
Smart Images

Figure CN118908432A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of corrosion inhibitors, in particular to a corrosion inhibitor for a cooling water system of a marine diesel engine and a preparation method and application thereof. Background Art
[0002] The cooling water system is one of the five major systems of a diesel engine. During the bench test of marine diesel engines, major diesel engine manufacturers face the following problems in the corrosion of the diesel engine cooling water system: 1. Complexity of the corrosive environment Water quality factors: During the production and manufacturing of diesel engines, metal dust, iron filings, oils, etc. in the casting process, as well as calcium and magnesium ions, chloride ions, sulfate ions, silicate ions, etc. in the cooling water accumulate in the cooling water system for a long time. These factors will accelerate the corrosion process of cooling water system components and increase the risk of corrosion.
[0003] Temperature fluctuation: During the bench test of the diesel engine, the temperature and pressure of the cooling water system will fluctuate with the test load requirements of the diesel engine. Under high temperature and high pressure conditions, the corrosion reaction of the cooling water system components will be accelerated, especially in the case of local overheating or cooling around the cylinder head and cylinder liner, the corrosion rate will be further increased.
[0004] 2. Diversity of corrosion types Electrochemical corrosion: The materials used in the cooling system are complex, including cast iron (alloy cast iron, vanadium-titanium cast iron, boron-added cast iron), cast steel, alloy steel, medium carbon steel, copper, brass, aluminum, aluminum alloy and solder, etc., as well as various non-metallic gaskets. When different metals are in a closed cooling water system, uniform micro-battery corrosion will occur; when two different metals come into contact with each other, due to the different corrosion potentials, the corrosion rate of the metal with a more negative corrosion potential increases, causing local corrosion at the contact point, that is, galvanic corrosion, and the electrochemical reaction of metal parts leads to the dissolution of the metal surface and the generation of corrosion products.
[0005] Chemical corrosion: Certain chemicals in cooling water (such as sulfate, chloride ions, etc.) will directly react chemically with metal parts, causing metal corrosion.
[0006] Cavitation (pitting) : When the diesel engine is running at high load, the impact and vibration of the diesel engine, the cooling water in the high-temperature components such as the cylinder liner and the local impact pressure, the cooling water will form many fine bubbles, which will burst on the surface of the metal parts, resulting in the formation of dense pitting-like cavities on the metal surface. Under high temperature and high pressure, the high-temperature chemical corrosion (oxygen diffusion) formed will cause the oxygen to corrode the metal parts again.
[0007] 3. Concentration of corrosion sites, such as Figure 1 shown.
[0008] Weak points of metal parts: such as cylinder liners, cylinder heads, water pump impellers and other parts, due to differences in materials and their complex internal structures, are very likely to become concentrated areas of high temperature and high pressure corrosion.
[0009] Areas with low cooling water flow rate: Impurities and corrosion products in the cooling water are easily deposited to form a scale layer, further aggravating corrosion. The deposition of corrosion products will block the cooling water channel, reduce the flow rate of the cooling water and the heat exchange efficiency, and cause the diesel engine to overheat.
[0010] The current solutions to the above problems include: improving the water quality and the material of the cooling water system or changing the operation of the cooling water system of the diesel engine test station by adding cooling water additives, but none of them can solve the corrosion problem of high temperature and high pressure.
[0011] Therefore, there is an urgent need to provide a corrosion inhibitor for a diesel engine cooling water system to solve the above technical problems. Summary of the invention
[0012] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a corrosion inhibitor.
[0013] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows: A corrosion inhibitor for a marine diesel engine cooling water system, comprising the following components by weight: 10-50 parts of methyldiethanolamine, 10-40 parts of monoethanolamine, 0.5-8 parts of hexadecylamine, 0.05-8 parts of benzotriazole, Polyaspartic acid 0.03-6 parts, Sodium polyacrylate 0.05-10 parts, 0.5-15 parts of terpolymeric acid, 3-20 parts of aliphatic dibasic acid, Neodecanoic acid 0.05-16 parts, Borax 0.5-18 parts, 0.1-15 parts of alkyl alcohol amide, 0.05-12 parts of propylene oxide condensate, Ethylene oxide condensation product 0.02-8 parts, 0.02-5 parts of phosphonocarboxylic acid copolymer, 2-phosphonobutane-1,2,4-tricarboxylic acid 0.05-9 parts, 5-20 parts of purified water.
[0014] Furthermore, the invention also comprises 0.03-12 parts of dicyclohexylamine nitrite.
[0015] Furthermore, the propylene oxide condensate is polyethylene glycol PEG200-6000, and the ethylene oxide condensate is polypropylene glycol PPG400-10000.
[0016] Furthermore, the preparation method comprises the following steps: Step S1: monoethanolamine and tribasic polycarboxylic acid are firstly neutralized to produce a neutral transparent liquid 1; monoethanolamine and aliphatic dibasic acid are firstly neutralized to produce a transparent neutral liquid 2; monoethanolamine, neodecanoic acid and borax are firstly neutralized to produce a transparent neutral liquid 3; monoethanolamine and benzotriazole are firstly neutralized to produce a transparent neutral liquid 4; Step S2: Add the transparent neutral liquid 1, transparent neutral liquid 2, transparent neutral liquid 3 and transparent neutral liquid 4 prepared in S1 into the reaction kettle respectively, heat and stir evenly, continue to add the remaining materials, and after all the materials are added, stir and mix at 75-85°C to obtain a weakly alkaline brown viscous liquid.
[0017] Furthermore, the heating temperature in step S2 is 75-85°C.
[0018] Furthermore, after all materials are added in step S2, stirring is performed for 3.5-4.5 hours. Application of the corrosion inhibitor in a diesel engine system.
[0019] The beneficial effects of the technical solution of the present invention are: The all-organic environmentally friendly corrosion inhibitor in the present invention is a composite film-forming corrosion inhibitor that combines a deposition film type and an adsorption film type. It contains functional groups such as N, S, P, and O, and contains hydrophilic groups that can be adsorbed on the metal surface and hydrophobic groups that shield the metal surface. The hydrophilic groups are directionally adsorbed on the metal surface, while the hydrophobic groups hinder the diffusion of water and dissolved oxygen to the metal, thereby achieving a corrosion inhibition effect. It can effectively inhibit the electrochemical corrosion of various metals in high-temperature cooling water; inhibit the chemical corrosion caused by chloride ions, silicate ions, and sulfate ions in cooling water; and inhibit cavitation (pitting) caused by the bursting of bubbles generated when the diesel engine is running at high load and the cooling water system is under high pressure and high temperature, including uniform corrosion and local corrosion (such as pitting, crevice corrosion, etc.).
[0020] The corrosion inhibitor in the present invention is stable under high pressure and high temperature conditions, is not easy to decompose, and forms an organic film on the metal surface, which can isolate the dissolved oxygen and corrosive ions in the water and prevent the cavitation of metal parts by the bursting of bubbles, thereby achieving a corrosion inhibition and protection effect. In addition, the corrosion inhibitor in the present invention also has the function of inhibiting microorganisms and bacteria in the cooling water system, which can prevent the decomposition and corrosion of microorganisms in the cooling water.
[0021] Scale is easily formed in high-temperature cooling water, especially in areas with high hardness water. Impurities and corrosion products in the cooling water are deposited to form a scale layer, further aggravating corrosion. Scale will also be deposited on the metal surface. The corrosion inhibitor in the present invention has a certain scale inhibition ability. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Schematic diagram of the corrosion of metal parts.
[0024] Figure 2 This is a schematic diagram of the corrosion condition of a diesel engine using the corrosion inhibitor of the present invention after 112 days of commissioning testing. DETAILED DESCRIPTION
[0025] The present invention will be further described below in conjunction with specific implementations and accompanying drawings.
[0026] Example 1 A corrosion inhibitor for a marine diesel engine cooling water system, comprising the following components by weight: 10 parts of methyldiethanolamine, 10 parts of monoethanolamine, 0.5 parts of hexadecylamine, 0.05 parts of benzotriazole, Polyaspartic acid 0.03 parts, 0.05 parts of sodium polyacrylate, 0.5 parts of terpolymeric carboxylic acid, 3 parts of aliphatic dibasic acid, Neodecanoic acid 0.05 parts, 0.5 parts of borax, 0.1 part of alkyl alcohol amide, 0.05 parts of propylene oxide condensate, 0.02 parts of ethylene oxide condensation product, 0.02 parts of phosphonocarboxylic acid copolymer, 0.05 parts of 2-phosphonobutane-1,2,4-tricarboxylic acid, 5 parts of purified water.
[0027] Among them, the propylene oxide condensate is polyethylene glycol PEG200-6000, and the ethylene oxide condensate is polypropylene glycol PPG400-10000.
[0028] The preparation method of the corrosion inhibitor in this embodiment comprises the following steps: Step S1: monoethanolamine and tribasic polycarboxylic acid are firstly neutralized to produce a neutral transparent liquid 1; monoethanolamine and aliphatic dibasic acid are firstly neutralized to produce a transparent neutral liquid 2; monoethanolamine, neodecanoic acid and borax are firstly neutralized to produce a transparent neutral liquid 3; monoethanolamine and benzotriazole are firstly neutralized to produce a transparent neutral liquid 4; Step S2: Add the transparent neutral liquid 1, transparent neutral liquid 2, transparent neutral liquid 3 and transparent neutral liquid 4 prepared in S1 into the reaction kettle respectively, heat to 75°C and stir evenly, continue to add the remaining materials, and after all the materials are added, stir at 75°C for 3.5 hours to obtain a weakly alkaline brown viscous liquid.
[0029] Example 2 A corrosion inhibitor for a marine diesel engine cooling water system, comprising the following components by weight: 30 parts of methyldiethanolamine, 25 parts of monoethanolamine, 4 parts of hexadecylamine, 4 parts of benzotriazole, 3 parts of polyaspartic acid, 5 parts of sodium polyacrylate, 7 parts of terpolymeric carboxylic acid, 12 parts of aliphatic dibasic acid, 8 parts of neodecanoic acid, 9 parts of borax, 8 parts of alkyl alcohol amide, 6 parts of propylene oxide condensate, 4 parts of ethylene oxide condensation product, 3 parts of phosphonocarboxylic acid copolymer, 5 parts of 2-phosphonobutane-1,2,4-tricarboxylic acid, 0.03 parts of dicyclohexylamine nitrite, 10 parts of purified water.
[0030] Among them, the propylene oxide condensate is polyethylene glycol PEG200-6000, and the ethylene oxide condensate is polypropylene glycol PPG400-10000.
[0031] The preparation method of the corrosion inhibitor in this embodiment comprises the following steps: Step S1: monoethanolamine and tribasic polycarboxylic acid are firstly neutralized to produce a neutral transparent liquid 1; monoethanolamine and aliphatic dibasic acid are firstly neutralized to produce a transparent neutral liquid 2; monoethanolamine, neodecanoic acid and borax are firstly neutralized to produce a transparent neutral liquid 3; monoethanolamine and benzotriazole are firstly neutralized to produce a transparent neutral liquid 4; Step S2: Add the transparent neutral liquid 1, transparent neutral liquid 2, transparent neutral liquid 3 and transparent neutral liquid 4 prepared in S1 into the reaction kettle respectively, heat to 80°C and stir evenly, continue to add the remaining materials, and after all the materials are added, stir at 80°C for 4 hours to obtain a weakly alkaline brown viscous liquid. Example 3 A corrosion inhibitor for a marine diesel engine cooling water system, comprising the following components by weight: 30 parts of methyldiethanolamine, 25 parts of monoethanolamine, 4 parts of hexadecylamine, 4 parts of benzotriazole, 3 parts of polyaspartic acid, 5 parts of sodium polyacrylate, 7 parts of terpolymeric carboxylic acid, 12 parts of aliphatic dibasic acid, 8 parts of neodecanoic acid, 9 parts of borax, 8 parts of alkyl alcohol amide, 6 parts of propylene oxide condensate, 4 parts of ethylene oxide condensation product, 3 parts of phosphonocarboxylic acid copolymer, 5 parts of 2-phosphonobutane-1,2,4-tricarboxylic acid, 6 parts of dicyclohexylamine nitrite, 12 parts of purified water.
[0033] Among them, the propylene oxide condensate is polyethylene glycol PEG200-6000, and the ethylene oxide condensate is polypropylene glycol PPG400-10000.
[0034] The preparation method of the corrosion inhibitor in this embodiment comprises the following steps: Step S1: monoethanolamine and tribasic polycarboxylic acid are firstly neutralized to produce a neutral transparent liquid 1; monoethanolamine and aliphatic dibasic acid are firstly neutralized to produce a transparent neutral liquid 2; monoethanolamine, neodecanoic acid and borax are firstly neutralized to produce a transparent neutral liquid 3; monoethanolamine and benzotriazole are firstly neutralized to produce a transparent neutral liquid 4; Step S2: Add the transparent neutral liquid 1, transparent neutral liquid 2, transparent neutral liquid 3 and transparent neutral liquid 4 prepared in S1 into the reaction kettle respectively, heat to 80°C and stir evenly, continue to add the remaining materials, and after all the materials are added, stir at 80°C for 4 hours to obtain a weakly alkaline brown viscous liquid. Example 4 A corrosion inhibitor for a marine diesel engine cooling water system, comprising the following components by weight: 30 parts of methyldiethanolamine, 25 parts of monoethanolamine, 4 parts of hexadecylamine, 4 parts of benzotriazole, 3 parts of polyaspartic acid, 5 parts of sodium polyacrylate, 7 parts of terpolymeric carboxylic acid, 12 parts of aliphatic dibasic acid, 8 parts of neodecanoic acid, 9 parts of borax, 8 parts of alkyl alcohol amide, 6 parts of propylene oxide condensate, 4 parts of ethylene oxide condensation product, 3 parts of phosphonocarboxylic acid copolymer, 5 parts of 2-phosphonobutane-1,2,4-tricarboxylic acid, 12 parts of dicyclohexylamine nitrite, 15 parts of purified water.
[0036] Among them, the propylene oxide condensate is polyethylene glycol PEG200-6000, and the ethylene oxide condensate is polypropylene glycol PPG400-10000.
[0037] The preparation method of the corrosion inhibitor in this embodiment comprises the following steps: Step S1: monoethanolamine and tribasic polycarboxylic acid are firstly neutralized to produce a neutral transparent liquid 1; monoethanolamine and aliphatic dibasic acid are firstly neutralized to produce a transparent neutral liquid 2; monoethanolamine, neodecanoic acid and borax are firstly neutralized to produce a transparent neutral liquid 3; monoethanolamine and benzotriazole are firstly neutralized to produce a transparent neutral liquid 4; Step S2: Add the transparent neutral liquid 1, transparent neutral liquid 2, transparent neutral liquid 3 and transparent neutral liquid 4 prepared in S1 into the reaction kettle respectively, heat to 80°C and stir evenly, continue to add the remaining materials, and after all the materials are added, stir at 80°C for 4 hours to obtain a weakly alkaline brown viscous liquid.
[0038] Example 5 A corrosion inhibitor for a marine diesel engine cooling water system, comprising the following components by weight: 50 parts of methyldiethanolamine, 40 parts of monoethanolamine, 8 parts of hexadecylamine, 8 parts of benzotriazole, 6 parts of polyaspartic acid, 10 parts of sodium polyacrylate, 15 parts of terpolymeric carboxylic acid, 20 parts of aliphatic dibasic acid, 16 parts of neodecanoic acid, 18 parts of borax, 15 parts of alkyl alcohol amide, 12 parts of propylene oxide condensate, 8 parts of ethylene oxide condensation product, 5 parts of phosphonocarboxylic acid copolymer, 9 parts of 2-phosphonobutane-1,2,4-tricarboxylic acid, 20 parts of purified water.
[0039] Among them, the propylene oxide condensate is polyethylene glycol PEG200-6000, and the ethylene oxide condensate is polypropylene glycol PPG400-10000.
[0040] The preparation method of the corrosion inhibitor in this embodiment comprises the following steps: Step S1: monoethanolamine and tribasic polycarboxylic acid are firstly neutralized to produce a neutral transparent liquid 1; monoethanolamine and aliphatic dibasic acid are firstly neutralized to produce a transparent neutral liquid 2; monoethanolamine, neodecanoic acid and borax are firstly neutralized to produce a transparent neutral liquid 3; monoethanolamine and benzotriazole are firstly neutralized to produce a transparent neutral liquid 4; Step S2: Add the transparent neutral liquid 1, transparent neutral liquid 2, transparent neutral liquid 3 and transparent neutral liquid 4 prepared in S1 into the reaction kettle respectively, heat to 85°C and stir evenly, continue to add the remaining materials, and after all the materials are added, stir at 85°C for 4.5 hours to obtain a weakly alkaline brown viscous liquid.
[0041] The corrosion inhibitors prepared in Examples 1-5 were tested for stability under high pressure and high temperature, and the test conditions were cooling water at 20 atmospheres and a temperature of about 200 degrees for 720 hours. The test results showed that none of the corrosion inhibitors decomposed or produced harmful substances, ensuring that the corrosion-slowing performance of the inhibitors was weakened or decomposed during long-term use.
[0042] Application testing: 12X92DF is the world's first dual-fuel marine diesel engine with the largest power and a new generation of control system. It was designed, manufactured and debugged by a domestic diesel engine manufacturer. This model is the world's first model, and the total test bench and debugging test lasted 112 days. During the testing phase, this type of diesel engine underwent multiple rounds of cylinder lifting and inspection. The cooling water performance indicators have been tested by long-term high-temperature, high-pressure operation and temperature changes in complex application environments. The scale and cavitation performance indicators of high-temperature parts have been fully verified through the status of disassembled and inspected parts. For details, see Figure 2 The corrosion protection effect of the cooling water system has been unanimously recognized by the main engine manufacturer and shipowner.
[0043] It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary experimental examples, and that the present invention can be implemented in other specific forms without departing from the spirit and essential features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention, and any reference numerals in the claims should not be regarded as limiting the claims involved.
[0044] In addition, it should be understood that although this specification is described according to implementation methods, not every implementation method contains only one independent claim scheme. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other implementation methods that can be understood by those skilled in the art.
Claims
1. A corrosion inhibitor for a marine diesel engine cooling water system, characterized in that: Its mass composition is as follows: 10-50 parts of methyldiethanolamine, 10-40 parts of monoethanolamine, 0.5-8 parts of hexadecylamine, 0.05-8 parts of benzotriazole, Polyaspartic acid 0.03-6 parts, Sodium polyacrylate 0.05-10 parts, 0.5-15 parts of terpolymeric acid, 3-20 parts of aliphatic dibasic acid, Neodecanoic acid 0.05-16 parts, Borax 0.5-18 parts, 0.1-15 parts of alkyl alcohol amide, 0.05-12 parts of propylene oxide condensate, Ethylene oxide condensation product 0.02-8 parts, 0.02-5 parts of phosphonocarboxylic acid copolymer, 2-phosphonobutane-1,2,4-tricarboxylic acid 0.05-9 parts, 5-20 parts of purified water.
2. The corrosion inhibitor for a marine diesel engine cooling water system according to claim 1, characterized in that: Its mass composition is as follows: 30 parts of methyldiethanolamine, 25 parts of monoethanolamine, 4 parts of hexadecylamine, 4 parts of benzotriazole, 3 parts of polyaspartic acid, 5 parts of sodium polyacrylate, 7 parts of terpolymeric carboxylic acid, 12 parts of aliphatic dibasic acid, 8 parts of neodecanoic acid, 9 parts of borax, 8 parts of alkyl alcohol amide, 6 parts of propylene oxide condensate, 4 parts of ethylene oxide condensation product, 3 parts of phosphonocarboxylic acid copolymer, 5 parts of 2-phosphonobutane-1,2,4-tricarboxylic acid, 6 parts of dicyclohexylamine nitrite, 12 parts of purified water.
3. The corrosion inhibitor for a marine diesel engine cooling water system according to claim 1, characterized in that: It also contains 0.03-12 parts of dicyclohexylamine nitrite.
4. The corrosion inhibitor for a marine diesel engine cooling water system according to claim 1, characterized in that: The propylene oxide condensate is polyethylene glycol PEG200-6000, and the ethylene oxide condensate is polypropylene glycol PPG400-10000.
5. The method for preparing a corrosion inhibitor for a marine diesel engine cooling water system according to claim 1, characterized in that: The preparation method comprises the following steps: Step S1: monoethanolamine and tribasic polycarboxylic acid are firstly neutralized to produce a neutral transparent liquid 1; monoethanolamine and aliphatic dibasic acid are firstly neutralized to produce a transparent neutral liquid 2; monoethanolamine, neodecanoic acid and borax are firstly neutralized to produce a transparent neutral liquid 3; monoethanolamine and benzotriazole are firstly neutralized to produce a transparent neutral liquid 4; Step S2: Add the transparent neutral liquid 1, transparent neutral liquid 2, transparent neutral liquid 3 and transparent neutral liquid 4 prepared in S1 into the reaction kettle respectively, heat and stir evenly, continue to add the remaining materials, and after all the materials are added, stir and mix at 75-85°C to obtain a weakly alkaline brown viscous liquid.
6. The method for preparing a corrosion inhibitor for a marine diesel engine cooling water system according to claim 5, characterized in that: The heating temperature in step S2 is 75-85°C.
7. The method for preparing a corrosion inhibitor for a marine diesel engine cooling water system according to claim 5, characterized in that: After all materials are added in step S2, stir for 3.5-4.5 hours.
8. Use of the corrosion inhibitor according to any one of claims 1 to 7 in a diesel engine system.
Citation Information
Cited By
Preparation method of corrosion and scale inhibitor
CN119570524A
Preparation method of corrosion and scale inhibitor
CN119570524B