Strong-sound-absorption open-cell foamed glass and preparation method thereof
By using sodium carbonate, sodium fluorosilicate and modified basalt fibers in foam glass, a complex pore structure is formed, which solves the problems of poor sound absorption and sound insulation effect of existing foam glass, and achieves high mechanical strength and excellent sound absorption capacity. .
Patent Information
- Application Number
- CN202411236031.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-08
AI Technical Summary
The sound absorption and sound insulation effects of existing foam glass are not satisfactory, and it is difficult to meet the needs of complex sound wave reflection and frictional viscosity.
Sodium carbonate, sodium fluorosilicate and modified basalt fibers are used as the constituent materials to generate gases by decomposing sodium carbonate at high temperatures, sodium fluorosilicate reduces the melting temperature of glass and sodium phosphate stabilizes bubbles, combining the load and surface modification of modified basalt fibers , forming complex pore structures to improve sound absorption and sound insulation effect.
The sound absorption and sound insulation effect of foam glass is significantly improved, mechanical strength and thermal isolation performance are enhanced, and the number of sound wave reflections and frictional viscosity are improved through complex pore structures and controlled ratios of open and closed pores, which is improved.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to a strong sound-absorbing open-hole foamed glass and a preparation method thereof. Background Art
[0002] Foam glass is a typical porous material with the characteristics of low density, light weight, high thermal resistance and high temperature resistance. It is widely used in construction, national defense and industry. The raw materials for preparing foam glass include a main raw material that can be vitrified at high temperature and a foaming agent that can release gas to form bubbles. The foaming process adopts a high-temperature sintering method. At the foaming temperature, the foaming agent releases gaseous substances due to its thermal decomposition or thermal activation reaction, forming bubbles in the softened glass, thereby forming foam glass.
[0003] Foam glass has attracted much attention due to its wide range of applications, such as separation process, bone regeneration, thermal and sound insulation, flame retardancy, high chemical resistance, etc. Due to its excellent physical and chemical properties, foam glass is widely used in the fields of petroleum, chemical industry, electric power, national defense and military industry, etc. It can also be directly used to make strange stones, large sculptures, various engineering components, green walls, etc. As a thermal insulation material, foam glass has excellent properties such as high strength, low thermal conductivity, water resistance, moisture resistance, and erosion resistance. It can be used in cold storage, underground oil pipelines, and walls and ceilings of various buildings to play a role in thermal insulation.
[0004] In the preparation process of foam glass, additives play an important role in the formation of bubbles and the stability of bubble structure. Commonly used additives are foaming agents, foam stabilizers and co-solvents. Different types of reagents play different roles in foam glass. Similarly, the effects on the pore structure and macroscopic physical properties of foam glass are also different.
[0005] Foaming agent refers to a substance that can promote the formation of pore structure in the batch. Foaming agents are generally divided into two categories: one is high-temperature self-decomposition, which can decompose and release oxygen, carbon dioxide, sulfur dioxide and other gases at high temperatures, such as carbonates (magnesium carbonate, calcium carbonate, sodium carbonate, dolomite powder, etc.), sulfates (glauber's salt, hard stone slurry, etc.) and manganese dioxide; the second is high-temperature chemical reaction, which can react with other substances at high temperatures to generate carbon dioxide, carbon monoxide and other gases, such as carbon black, carbon powder, limestone, magnesite, silicon carbide, aluminum powder, etc.
[0006] Stabilizers can also be called modifiers. Adding an appropriate amount of foam stabilizer can improve the performance of foam glass, increase the foaming temperature range, reduce the number of interconnected holes, and improve the thermal insulation performance, mechanical strength and product yield. Currently used foam stabilizers include sodium hexametaphosphate, boric acid, iron oxide, sodium phosphate, titanate trioxide, borax, sodium pyrophosphate, sodium sulfate, etc.
[0007] In the production process of foam glass, flux is also an important additive. During the main heating process, the softening temperature is reduced so that it can be completely softened when the foaming agent reacts and releases gas. Usually, a certain amount of flux is added. Because when the temperature reaches the melting temperature of the glass, the foaming agent begins to react slowly, and the generated gas will escape from the gap of the unmelted mixture. Only by properly lowering the melting temperature of the mixture and ensuring that the mixture is completely softened to a molten state before a large amount of foaming gas is generated, can better quality foam glass be obtained.
[0008] Chinese patent document CN107265871A discloses an energy-saving foam glass and a preparation method thereof. The foam glass comprises the following raw materials in parts by weight: 80-120 parts of cullet, 10-20 parts of silicon dioxide, 0.5-3 parts of sodium sulfate, 0.2-0.8 parts of sodium carbonate, 2-6 parts of calcium oxide, 0.5-2 parts of magnesium oxide, 0.2-0.8 parts of phosphorus pentoxide, 1-5 parts of coarse borax, 0.2-0.6 parts of antimony trioxide, 3-8 parts of foaming agent, and 1-3 parts of dispersant; the preparation method comprises three steps of processing cullet, mixing, and preheating, sintering, and foaming.
[0009] The sound insulation effect of foam glass is determined by the open bubbles inside, but the sound absorption and sound insulation effects of existing foam glass are unsatisfactory. Summary of the invention
[0010] In order to solve the deficiencies in the prior art, the object of the present invention is to provide a highly sound-absorbing open-pore foamed glass and a preparation method thereof. The prepared foamed glass has high mechanical strength and a complex pore structure, which can significantly increase the number of reflections of incident sound waves and the friction and viscosity effect, thereby improving the sound absorption and sound insulation effects of the foamed glass.
[0011] In order to achieve the above object, the present invention adopts the following technical solution: A highly sound-absorbing open-cell foamed glass is prepared from the following components by weight: 90-95 parts of glass powder, 1-5 parts of sodium carbonate, 3-5 parts of sodium fluorosilicate, 3-5 parts of sodium phosphate, and 2-6 parts of modified basalt fiber.
[0012] Preferably, the method for preparing the modified basalt fiber comprises the following steps: (1) soaking the basalt fiber in anhydrous ethanol, then washing it in acetone, filtering it and drying it to obtain pretreated basalt fiber; (2) adding the pretreated basalt fiber to a potassium permanganate solution, stirring the reaction, filtering and drying the product, and obtaining manganese dioxide-loaded basalt fiber; (3) Dispersing manganese dioxide-loaded basalt fiber and tetraethyl orthosilicate in anhydrous ethanol, adding ammonia water to adjust the pH, filtering and drying the product to obtain the modified basalt fiber.
[0013] Preferably, in step (1), the basalt fiber has a single filament diameter of 7-13 μm, a length of 5-25 mm, an elastic modulus of 95-115 GPa, a tensile strength of 3300-4500 MPa, an elongation at break of 2.4%-3.0%, and a density of 2.6-2.8 g·cm -3 .
[0014] Preferably, in step (1), the sample is immersed in anhydrous ethanol for 2 to 3 hours and then washed in acetone for 12 to 18 hours.
[0015] Specifically, in step (1), the immersion time in anhydrous ethanol can be 2 h, 2.5 h, or 3 h; the cleaning time in acetone can be 12 h, 13 h, 14 h, 15 h, 16 h, 17 h, or 18 h.
[0016] Preferably, in step (2), the concentration of the potassium permanganate solution is 2wt%~5wt%; and the dosage ratio of the pretreated basalt fiber to the potassium permanganate solution is 10g:50~100mL.
[0017] Preferably, in step (2), the stirring reaction condition is to keep the reaction at 50-60° C. for 4-6 hours.
[0018] Specifically, in step (2), the stirring reaction temperature can be 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C, or 60°C; and the reaction time can be 4h, 4.5h, 5h, 5.5h, or 6h.
[0019] Preferably, in step (3), the dosage ratio of manganese dioxide loaded basalt fiber, tetraethyl orthosilicate, and anhydrous ethanol is 10 g: 3-8 g: 100 mL.
[0020] Preferably, in step (3), the pH is adjusted to 7-11 with aqueous ammonia.
[0021] Specifically, in step (3), the pH is adjusted to 7, 8, 9, 10, or 11 with aqueous ammonia.
[0022] Preferably, the raw materials and mass fractions of the glass powder are as follows: 55.3-61.6 parts SiO 2 , 13.3~18.6 parts Na 2 CO 3 , 9.0~11.6 parts CaCO 3 , 5~5.7 parts Al 2 O 3 、3.56~5.8 parts MgCO 3 , 0.73~3.7 parts K 2 CO 3、0.51~1.2 parts Fe 2 O 3 , 0.53~1.1 parts BaCO 3 , 0.47~0.9 parts Na 2 SO 4 , 0.05~0.3 parts SrO.
[0023] More preferably, the raw materials and mass fractions of the glass powder are as follows: 58.45 parts SiO 2 , 15.95 parts Na 2 CO 3 , 10.3 parts CaCO 3 , 5.35 parts Al 2 O 3 、4.68 parts MgCO 3 , 2.215 copies of K 2 CO 3 、0.855 parts of Fe 2 O 3 , 0.815 parts of BaCO 3 , 0.685 parts Na 2 SO 4 , 0.175 parts SrO.
[0024] Preferably, the preparation method of the glass powder is as follows: the raw material of the glass powder is placed in a ball mill for dry grinding, and then melted at 1100-1300°C after dry grinding for 3-6 hours, and immediately quenched with water after being taken out of the furnace, and then dried and dry ground for 3-6 hours, and passed through a 140-200 mesh sieve to obtain the glass powder.
[0025] The present invention also claims a method for preparing the highly sound-absorbing open-cell foamed glass, comprising the following steps: a. Weigh the raw materials according to the mass ratio, send the glass powder, sodium carbonate, sodium fluorosilicate, sodium phosphate and modified basalt fiber to a grinder and grind and mix them to 200-250 meshes to obtain a mixture; b. The mixture is loaded into a mold, vibrated and mixed evenly, and then placed in a hot isostatic pressing furnace and evacuated, preheated at 550-600° C. for 20-40 min, then heated to 950-1050° C. at a rate of 50-80° C. / min, and foamed for 40-80 min; then cooled to 550-600° C., kept warm for 20-40 min for annealing, and finally cooled to below 100° C. at a rate of 2-3° C. / min to obtain the highly sound-absorbing open-cell foamed glass.
[0026] The foaming principle of sodium carbonate is as follows: Na 2 CO 3 →NaO+CO 2 ↑; Na 2 CO3 +SiO 2 →Na 2 SiO 3 +CO 2 ↑.
[0027] In an oxygen-free environment, the mixture undergoes a staged heating process. First, the temperature is slowly raised to 550-600°C and maintained for 20-40 minutes. This preheating stage is used to remove bound water and volatile substances in the green body. Subsequently, the temperature is quickly raised to 950-1050°C and maintained for 40-80 minutes for sintering and oxygen-free foaming. During the entire process, continuous exhaust is performed to ensure that the hot isostatic pressing furnace maintains an oxygen-free negative pressure state.
[0028] In this environment, sodium carbonate acts as a foaming agent to produce a bubble structure in the green body. At the same time, due to the high temperature and negative pressure conditions, the fluidity of the glass melt is enhanced, and the viscosity and interfacial tension are reduced. This allows the gas in the green body to expand in the bubbles, causing the bubbles to grow larger and the bubble walls to become thinner.
[0029] As the foaming process progresses, small bubbles gradually merge to form large bubbles, and tend to expand outward. The bubbles close to the surface of the green body may break through the bubble wall and form open holes due to the pressure difference between the inside and outside. This series of changes eventually leads to the formation of a porous structure and produces a large open porosity.
[0030] Compared with the prior art, the present invention has the following beneficial effects: 1) The present invention provides a highly sound-absorbing open-pore foamed glass. Sodium carbonate is used as a foaming agent, which decomposes at high temperature to generate gas and form a uniform pore structure, which is helpful to improve the sound absorption performance of the material; sodium fluorosilicate is used as a flux, which can reduce the melting temperature of the glass, is conducive to the foaming process, and can also reduce energy consumption; sodium phosphate is used as a foam stabilizer, which can stabilize the bubbles formed in the foaming process, prevent the bubbles from bursting or merging too quickly, and help form a uniform and stable pore structure; at the same time, modified basalt fiber is added, which can not only play a role in assisting foaming, but also improve the strength of the foamed glass products; the prepared foamed glass shows good mechanical strength, excellent compression resistance and bending resistance, thanks to the complex pore structure and controllable open and closed pore ratio, the material has excellent sound wave absorption ability, and also brings excellent thermal insulation performance.
[0031] 2) The present invention provides a modified basalt fiber. First, the basalt fiber is cleaned with anhydrous ethanol and acetone, and then potassium permanganate is used to generate manganese dioxide particles in situ on the basalt fiber to improve the surface performance of the basalt fiber, which is beneficial to the subsequent loading of silicon dioxide nanoparticles and improves the adhesion effect of silicon dioxide particles. Finally, the basalt fiber is modified with ethyl orthosilicate, which can generate more rough structures on the surface of the basalt fiber, on the one hand, increase the compatibility of the basalt fiber and the glass powder, so that the basalt fiber can be evenly dispersed in the glass powder, and on the other hand, it can also improve the bonding ability between the fiber and the glass matrix. In addition, manganese dioxide will undergo a decomposition reaction at high temperature. 4MnO 2 =2Mn 2 O 3 +O 2 , generating gas, which can be used as an auxiliary foaming agent. After in-situ loading of manganese dioxide modified basalt fiber, after high-temperature sintering, it can not only form an overlap structure to improve the strength of foam glass products, but also some fibers attached to the pore wall will enhance the structural stability of the pore wall and reduce the collapse of internal bubbles during sintering; at the same time, the manganese dioxide loaded on the surface of the modified basalt fiber will form bubbles along the fiber after decomposition, making the generated pores irregular or elongated, and even producing some directional pore structures, thereby affecting the connectivity of the bubbles and the ratio of open and closed pores, and significantly increasing the complexity of the pore structure of the foam glass, and increasing the number of reflections of the incident sound wave and the friction and viscosity through the maze effect, so that the kinetic energy of air movement is converted into heat energy and dissipated, thereby generating friction loss to attenuate the sound energy, and significantly improving the sound absorption and sound insulation effects of the material. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solution and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiments. Of course, the specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.
[0033] Unless otherwise specified, the chemical reagents and materials in the present invention are purchased from commercial sources or synthesized from raw materials purchased from commercial sources.
[0034] The present invention will be further described below through specific embodiments.
[0035] Example 1 A method for preparing highly sound-absorbing open-cell foamed glass comprises the following steps: (1) Soaking the basalt fiber in anhydrous ethanol for 3 hours, then washing it in acetone for 18 hours, filtering it and drying it to obtain pretreated basalt fiber; (2) Add 10 g of pretreated basalt fiber to 100 mL of 5 wt% potassium permanganate solution, stir and react at 60 °C for 4 h, filter and dry the product to obtain manganese dioxide-loaded basalt fiber; (3) Dispersing 10 g of manganese dioxide-loaded basalt fiber and 8 g of tetraethyl orthosilicate in 100 mL of anhydrous ethanol, adding ammonia water to adjust the pH to 11, filtering and drying the product to obtain modified basalt fiber; (4) 58.45 kg SiO 2 、15.95kg Na 2 CO 3 、10.3kg CaCO 3 , 5.35kg Al 2 O 3 、4.68kgMgCO 3 , 2.215kg K 2 CO 3 , 0.855kg Fe 2 O 3 , 0.815kg BaCO 3 , 0.685kg Na 2 SO 4 0.175 kg SrO was put into a ball mill for dry grinding. After dry grinding for 5 hours, it was melted at 1200°C, quenched with water immediately after being taken out of the furnace, dried and dry ground for 5 hours, and passed through a 150-mesh sieve to obtain glass powder. (5) Weigh the raw materials according to the mass ratio, and send 93 kg of glass powder, 3 kg of sodium carbonate, 4 kg of sodium fluorosilicate, 4 kg of sodium phosphate, and 6 kg of modified basalt fiber to a grinder for grinding and mixing to 220 mesh to obtain a mixture; (6) The mixture is placed in a mold, vibrated and mixed evenly, and then placed in a hot isostatic pressing furnace and evacuated. It is preheated at 600°C for 20 minutes, and then heated to 1050°C at a rate of 80°C / min and foamed for 40 minutes. The mixture is then cooled to 600°C and kept at this temperature for 40 minutes for annealing. Finally, it is cooled to below 100°C at a rate of 3°C / min to obtain a highly sound-absorbing open-cell foamed glass.
[0036] Example 2 A method for preparing highly sound-absorbing open-cell foamed glass comprises the following steps: (1) Soaking the basalt fiber in anhydrous ethanol for 2.5 hours, then washing it in acetone for 16 hours, filtering it and drying it to obtain pretreated basalt fiber; (2) Add 10 g of pretreated basalt fiber to 100 mL of 4 wt% potassium permanganate solution, stir and react at 55 °C for 5 h, filter and dry the product to obtain manganese dioxide-loaded basalt fiber; (3) Dispersing 10 g of manganese dioxide-loaded basalt fiber and 7 g of tetraethyl orthosilicate in 100 mL of anhydrous ethanol, adding ammonia water to adjust the pH to 10, filtering and drying the product to obtain modified basalt fiber; (4) 58.45 kg SiO 2 、15.95kg Na 2 CO 3 、10.3kg CaCO 3 , 5.35kg Al 2 O 3 、4.68kgMgCO 3 , 2.215kg K 2 CO 3 , 0.855kg Fe 2 O 3 , 0.815kg BaCO 3 , 0.685kg Na 2 SO 4 0.175 kg SrO was put into a ball mill for dry grinding. After dry grinding for 5 hours, it was melted at 1200°C, quenched with water immediately after being taken out of the furnace, dried and dry ground for 5 hours, and passed through a 150-mesh sieve to obtain glass powder. (5) Weigh the raw materials according to the mass ratio, and send 93 kg of glass powder, 3 kg of sodium carbonate, 4 kg of sodium fluorosilicate, 4 kg of sodium phosphate, and 5 kg of modified basalt fiber to a grinder for grinding and mixing to 220 mesh to obtain a mixed material; (6) The mixture is placed in a mold, vibrated and mixed evenly, and then placed in a hot isostatic pressing furnace and evacuated. It is preheated at 580°C for 30 min, then heated to 1020°C at a rate of 70°C / min and foamed for 50 min. The mixture is then cooled to 580°C and kept at this temperature for 30 min for annealing. Finally, the mixture is cooled to below 100°C at a rate of 2.5°C / min to obtain a highly sound-absorbing open-cell foamed glass.
[0037] Example 3 A method for preparing highly sound-absorbing open-cell foamed glass comprises the following steps: (1) Soaking the basalt fiber in anhydrous ethanol for 2.5 hours, then washing it in acetone for 14 hours, filtering it and drying it to obtain pretreated basalt fiber; (2) Add 10 g of pretreated basalt fiber to 100 mL of 3 wt% potassium permanganate solution, stir and react at 55 °C for 5 h, filter and dry the product to obtain manganese dioxide-loaded basalt fiber; (3) Dispersing 10 g of manganese dioxide-loaded basalt fiber and 5 g of tetraethyl orthosilicate in 100 mL of anhydrous ethanol, adding ammonia water to adjust the pH to 9, filtering and drying the product to obtain modified basalt fiber; (4) 58.45 kg SiO 2 、15.95kg Na 2 CO 3 、10.3kg CaCO 3 , 5.35kg Al 2 O 3 、4.68kgMgCO 3 , 2.215kg K 2 CO 3 , 0.855kg Fe 2 O 3 , 0.815kg BaCO 3 , 0.685kg Na 2 SO 4 0.175 kg SrO was put into a ball mill for dry grinding. After dry grinding for 5 hours, it was melted at 1200°C, quenched with water immediately after being taken out of the furnace, dried and dry ground for 5 hours, and passed through a 150-mesh sieve to obtain glass powder. (5) Weigh the raw materials according to the mass ratio, and send 93 kg of glass powder, 3 kg of sodium carbonate, 4 kg of sodium fluorosilicate, 4 kg of sodium phosphate, and 4 kg of modified basalt fiber to a grinder for grinding and mixing to 220 mesh to obtain a mixed material; (6) The mixture is placed in a mold, vibrated and mixed until uniformly mixed, and then placed in a hot isostatic pressing furnace and evacuated. It is preheated at 560°C for 30 min, and then heated to 1000°C at a rate of 60°C / min and foamed for 60 min. The mixture is then cooled to 570°C and kept at this temperature for 30 min for annealing. Finally, the mixture is cooled to below 100°C at a rate of 2.5°C / min to obtain a highly sound-absorbing open-cell foamed glass.
[0038] Example 4 A method for preparing highly sound-absorbing open-cell foamed glass comprises the following steps: (1) Soaking the basalt fiber in anhydrous ethanol for 2 hours, then washing it in acetone for 12 hours, filtering it and drying it to obtain pretreated basalt fiber; (2) Add 10 g of pretreated basalt fiber to 100 mL of 2 wt% potassium permanganate solution, stir and react at 50 °C for 6 h, filter and dry the product to obtain manganese dioxide-loaded basalt fiber; (3) Dispersing 10 g of manganese dioxide-loaded basalt fiber and 3 g of tetraethyl orthosilicate in 100 mL of anhydrous ethanol, adding ammonia water to adjust the pH to 7, filtering and drying the product to obtain modified basalt fiber; (4) 58.45 kg SiO 2 、15.95kg Na 2 CO 3 、10.3kg CaCO 3, 5.35kg Al 2 O 3 、4.68kgMgCO 3 , 2.215kg K 2 CO 3 , 0.855kg Fe 2 O 3 , 0.815kg BaCO 3 , 0.685kg Na 2 SO 4 0.175 kg SrO was put into a ball mill for dry grinding. After dry grinding for 5 hours, it was melted at 1200°C, quenched with water immediately after being taken out of the furnace, dried and dry ground for 5 hours, and passed through a 150-mesh sieve to obtain glass powder. (5) Weigh the raw materials according to the mass ratio, and send 93 kg of glass powder, 3 kg of sodium carbonate, 4 kg of sodium fluorosilicate, 4 kg of sodium phosphate, and 2 kg of modified basalt fiber to a grinder for grinding and mixing to 220 mesh to obtain a mixed material; (6) The mixture is placed in a mold, vibrated and mixed evenly, and then placed in a hot isostatic pressing furnace and evacuated. It is preheated at 550°C for 20 minutes, and then heated to 950°C at a rate of 50°C / min and foamed for 40 minutes. The mixture is then cooled to 550°C and kept at this temperature for 40 minutes for annealing. Finally, it is cooled to below 100°C at a rate of 2°C / min to obtain a highly sound-absorbing open-cell foamed glass.
[0039] Comparative Example 1 A method for preparing open-cell foamed glass comprises the following steps: (1) Soaking the basalt fiber in anhydrous ethanol for 3 hours, then washing it in acetone for 18 hours, filtering it and drying it to obtain pretreated basalt fiber; (2) Add 10 g of pretreated basalt fiber to 100 mL of 5 wt% potassium permanganate solution, stir and react at 60 °C for 4 h, filter and dry the product to obtain manganese dioxide-loaded basalt fiber; (3) 58.45 kg SiO 2 、15.95kg Na 2 CO 3 、10.3kg CaCO 3 , 5.35kg Al 2 O 3 、4.68kgMgCO 3 , 2.215kg K 2 CO 3 , 0.855kg Fe 2 O 3 , 0.815kg BaCO 3 , 0.685kg Na 2SO 4 0.175 kg SrO was put into a ball mill for dry grinding. After dry grinding for 5 hours, it was melted at 1200°C, quenched with water immediately after being taken out of the furnace, dried and dry ground for 5 hours, and passed through a 150-mesh sieve to obtain glass powder. (4) Weighing raw materials according to mass ratio, 93 kg of glass powder, 3 kg of sodium carbonate, 4 kg of sodium fluorosilicate, 4 kg of sodium phosphate, and 6 kg of manganese dioxide-loaded basalt fiber were sent to a grinder for grinding and mixing to 220 mesh to obtain a mixture; (5) The mixture is placed in a mold, vibrated and mixed evenly, and then placed in a hot isostatic pressing furnace and evacuated. It is preheated at 600°C for 20 min, then heated to 1050°C at a rate of 80°C / min and foamed for 40 min. The mixture is then cooled to 600°C and kept at this temperature for 40 min for annealing. Finally, it is cooled to below 100°C at a rate of 3°C / min to obtain an open-pore foamed glass.
[0040] Comparative Example 2 A method for preparing open-cell foamed glass comprises the following steps: (1) Soaking the basalt fiber in anhydrous ethanol for 3 hours, then washing it in acetone for 18 hours, filtering it and drying it to obtain pretreated basalt fiber; (2) 58.45 kg SiO 2 、15.95kg Na 2 CO 3 、10.3kg CaCO 3 , 5.35kg Al 2 O 3 、4.68kgMgCO 3 , 2.215kg K 2 CO 3 , 0.855kg Fe 2 O 3 , 0.815kg BaCO 3 , 0.685kg Na 2 SO 4 0.175 kg SrO was put into a ball mill for dry grinding. After dry grinding for 5 hours, it was melted at 1200°C, quenched with water immediately after being taken out of the furnace, dried and dry ground for 5 hours, and passed through a 150-mesh sieve to obtain glass powder. (3) Weighing raw materials according to mass ratio, sending 93 kg of glass powder, 3 kg of sodium carbonate, 4 kg of sodium fluorosilicate, 4 kg of sodium phosphate, and 6 kg of pretreated basalt fiber to a grinder and crushing and mixing them to 220 mesh to obtain a mixture; (4) The mixture is placed in a mold, vibrated and mixed evenly, and then placed in a hot isostatic pressing furnace and evacuated. It is preheated at 600°C for 20 min, then heated to 1050°C at a rate of 80°C / min and foamed for 40 min; then cooled to 600°C and kept at this temperature for 40 min for annealing. Finally, it is cooled to below 100°C at a rate of 3°C / min to obtain an open-pore foamed glass.
[0041] Comparative Example 3 A method for preparing highly sound-absorbing open-cell foamed glass comprises the following steps: (1) 58.45 kg SiO 2 、15.95kg Na 2 CO 3 、10.3kg CaCO 3 , 5.35kg Al 2 O 3 、4.68kgMgCO 3 , 2.215kg K 2 CO 3 , 0.855kg Fe 2 O 3 , 0.815kg BaCO 3 , 0.685kg Na 2 SO 4 0.175 kg SrO was put into a ball mill for dry grinding. After dry grinding for 5 hours, it was melted at 1200°C, quenched with water immediately after being taken out of the furnace, dried and dry ground for 5 hours, and passed through a 150-mesh sieve to obtain glass powder. (2) Weighing raw materials according to mass proportion, 93 kg of glass powder, 3 kg of sodium carbonate, 4 kg of sodium fluorosilicate, 4 kg of sodium phosphate, and 2 kg of manganese dioxide are sent to a grinder and crushed and mixed to 220 mesh to obtain a mixed material; (3) The mixture is placed in a mold, vibrated and mixed evenly, and then placed in a hot isostatic pressing furnace and evacuated. It is preheated at 600°C for 20 min, then heated to 1050°C at a rate of 80°C / min and foamed for 40 min. The mixture is then cooled to 600°C and kept at this temperature for 40 min for annealing. Finally, it is cooled to below 100°C at a rate of 3°C / min to obtain an open-pore foamed glass.
[0042] The foamed glasses obtained in Examples 1 to 4 and Comparative Examples 1 to 3 were prepared into plate-shaped samples with a size of 200 mm×200 mm×25 mm. The compressive strength and open porosity of the samples were tested with reference to JC / T 647-2014 “Foamed glass insulation products”. The sound absorption coefficient of the samples was tested with reference to GB / T 18696.1-2004 “Measurement of sound absorption coefficient and acoustic impedance in acoustic impedance tubes Part 1: Standing wave ratio method”. Three samples were prepared repeatedly for each example, and the test results were averaged. The results are shown in Table 1.
[0043] Table 1 Test results of open-cell foamed glass performance
[0044] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A strong sound-absorbing open-cell foamed glass, characterized in that: The invention is made of the following components in parts by weight: 90-95 parts of glass powder, 1-5 parts of sodium carbonate, 3-5 parts of sodium fluorosilicate, 3-5 parts of sodium phosphate and 2-6 parts of modified basalt fiber.
2. The strong sound-absorbing open-cell foamed glass according to claim 1, characterized in that: The preparation method of the modified basalt fiber comprises the following steps: (1) soaking the basalt fiber in anhydrous ethanol, then washing it in acetone, filtering it and drying it to obtain pretreated basalt fiber; (2) adding the pretreated basalt fiber to a potassium permanganate solution, stirring the reaction, filtering and drying the product, and obtaining manganese dioxide-loaded basalt fiber; (3) Dispersing manganese dioxide loaded basalt fiber and tetraethyl orthosilicate in anhydrous ethanol, adding ammonia water to adjust the pH, filtering and drying the product to obtain the modified basalt fiber.
3. The strong sound-absorbing open-cell foamed glass according to claim 2, characterized in that: In step (1), soak in anhydrous ethanol for 2 to 3 hours and clean in acetone for 12 to 18 hours.
4. The strong sound-absorbing open-cell foamed glass according to claim 2, characterized in that: In step (2), the concentration of the potassium permanganate solution is 2wt%~5wt%; the dosage ratio of the pretreated basalt fiber and the potassium permanganate solution is 10g:50~100mL.
5. The strong sound-absorbing open-cell foamed glass according to claim 2, characterized in that: In step (2), the stirring reaction conditions are 50-60° C. and the reaction is kept warm for 4-6 hours.
6. The strong sound-absorbing open-cell foamed glass according to claim 2, characterized in that: In step (3), the dosage ratio of manganese dioxide loaded basalt fiber, tetraethyl orthosilicate, and anhydrous ethanol is 10 g: 3-8 g: 100 mL.
7. The strong sound-absorbing open-cell foamed glass according to claim 2, characterized in that: In step (3), the pH is adjusted to 7-11 with aqueous ammonia.
8. The strong sound-absorbing open-cell foamed glass according to claim 1, characterized in that: The raw materials and mass proportions of the glass powder are as follows: 55.3~61.6 parts of SiO2, 13.3~18.6 parts of Na2CO3, 9.0~11.6 parts of CaCO3, 5~5.7 parts of Al2O3, 3.56~5.8 parts of MgCO3, 0.73~3.7 parts of K2CO3, 0.51~1.2 parts of Fe2O3, 0.53~1.1 parts of BaCO3, 0.47~0.9 parts of Na2SO4, and 0.05~0.3 parts of SrO.
9. The strong sound-absorbing open-cell foamed glass according to claim 8, characterized in that: The preparation method of the glass powder is as follows: the raw material of the glass powder is put into a ball mill for dry grinding, and then melted at 1100-1300° C. after dry grinding for 3-6 hours, and immediately quenched with water after being taken out of the furnace, and then dried and dry ground for 3-6 hours, and passed through a 140-200 mesh sieve to obtain the glass powder.
10. A method for preparing the highly sound-absorbing open-cell foamed glass according to any one of claims 1 to 9, characterized in that: The steps include: a. Weigh the raw materials according to the mass ratio, send the glass powder, sodium carbonate, sodium fluorosilicate, sodium phosphate and modified basalt fiber to a grinder and grind and mix them to 200-250 meshes to obtain a mixture; b. The mixture is loaded into a mold, vibrated and mixed evenly, and then put into a hot isostatic pressing furnace and evacuated, preheated at 550-600° C. for 20-40 min, then heated to 950-1050° C. at a rate of 50-80° C. / min, and foamed for 40-80 min; then cooled to 550-600° C., kept warm for 20-40 min for annealing, and finally cooled to below 100° C. at a rate of 2-3° C. / min to obtain the highly sound-absorbing open-cell foamed glass.