Powdery cement grinding aid for promoting cement grinding

By using powdered cement aids of dodecyl aminopropionate, montmorillonite, nanosilica, medium calcium fly ash and additives, concrete caused by the increase in sulfate in cement in the prior art is solved. The problem of structural deterioration has achieved the effect of improving cement grinding efficiency and concrete compressive strength.

CN118908613APending Publication Date: 2024-11-08GUANGXI HANHUA ARCHITECTURAL DESIGN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310499014.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-06
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Yuanming powder used in existing powdered cement aids leads to an increase in sulfate in cement, resulting in deterioration and failure of concrete structure.

Method used

Powdered cement-assisted grinding consisting of methyl dodecyl aminopropionate, montmorillonite, nanosilica, medium calcium fly ash and additives such as polyacrylamide, boric acid, nano calcium silicate and silane The agent improves the cement grinding effect and the compressive strength of concrete through the preparation of medium calcium fly ash and the synergistic effect of additives.

Benefits of technology

It significantly improves the cement grinding efficiency and compressive strength of concrete, reduces sulfate corrosion, extends the service life of concrete, and improves the grinding effect and powder selection efficiency of the ball mill, reducing grinding energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004213105010000081
    Figure BDA0004213105010000081
  • Figure BDA0004213105010000091
    Figure BDA0004213105010000091
  • Figure BDA0004213105010000092
    Figure BDA0004213105010000092
Patent Text Reader

Abstract

The invention discloses a powdery cement grinding aid for promoting cement grinding, which is characterized by being mainly prepared from the following raw materials: methyl dodecyl aminopropionate, montmorillonite, nano silicon dioxide, medium-calcium fly ash and an additive, the preparation method of the medium-calcium fly ash comprises the following steps: uniformly mixing calcium carbonate, calcium chloride and fly ash, and calcining at 1300-1500 DEG C for a period of time to obtain the medium-calcium fly ash. According to the powdery cement grinding aid for promoting cement grinding, all the raw material components play a synergistic and complementary role, the grinding effect and the grinding speed of cement in the grinding process are improved, the energy consumption of a ball mill is reduced, and the cement grinding cost is reduced. Meanwhile, cement prepared from the powdery cement grinding aid is good in compressive strength and cracking resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, in particular to a powdered cement grinding aid for promoting cement grinding. Background Art

[0002] Cement grinding is the last process of cement manufacturing. The particle size of cement grinding determines the quality of cement. The cement crushing process is that the material is denatured under a certain pressure. After the material accumulates a certain amount of energy, cracks are generated. After the cracks continue to expand, the material is crushed. In the process of material crushing, a lot of energy is consumed. Cement grinding aid is a chemical additive that improves the effect and performance of cement grinding. It has the effect of significantly improving the cement hourly output, cement strength at all ages, and improving cement fluidity. Cement grinding aid can greatly reduce the electrostatic adsorption ball phenomenon formed during the grinding process, and can reduce the re-agglomeration trend of ultrafine particles formed during the grinding process. Cement grinding aid can also significantly improve the fluidity of cement, improve the grinding effect of the ball mill and the powder selection efficiency of the powder selector, and reduce the energy consumption of grinding. At the same time, it can cover the distribution of cement particles and stimulate the hydration power, thereby improving the early strength and late strength of cement. Therefore, in the process of cement grinding, adding cement grinding aid has a great influence on the performance of cement.

[0003] However, current powdered cement grinding aids mostly use sodium sulfate as the main raw material, which causes an increase in sulfate in cement and ultimately an increase in sulfate in concrete. Too much sulfate in concrete will form sulfate erosion and cause the concrete structure to deteriorate and fail.

[0004] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0005] The object of the present invention is to provide a powdered cement grinding aid for promoting cement grinding, thereby overcoming the problem that the existing powdered cement grinding aid causes an increase in sulfate in cement, and when the cement is used, sulfate erosion causes concrete structure deterioration and failure.

[0006] In order to obtain a powdered cement grinding aid for promoting cement grinding, the present application provides a cement using the powdered cement grinding aid.

[0007] To achieve the above objectives, the present application first provides a powdered cement grinding aid for promoting cement grinding, using the following technical solution:

[0008] A powdered cement grinding aid for promoting cement grinding, wherein the grinding aid is mainly made of the following raw materials: methyl dodecylaminopropionate, montmorillonite, nano silicon dioxide, medium calcium fly ash, and additives; the medium calcium fly ash is prepared by the following method: mixing calcium carbonate, calcium chloride and fly ash, and calcining them at a temperature of 1300-1500°C for a period of time to obtain the medium calcium fly ash.

[0009] Preferably, in the above technical solution, the preparation method of the medium-calcium fly ash is as follows: calcium carbonate, calcium chloride and fly ash are mixed and calcined at 1300-1500°C for 6-8h, and after calcination, the mixture is ground and sieved to obtain a material with a particle size of ≤8mm.

[0010] Preferably, in the above technical solution, the ratio of raw materials required for the medium-calcium fly ash preparation method is: 11.5-19.4% calcium carbonate, 0.1-0.5% calcium chloride and 80-88.4% fly ash, calculated by weight percentage.

[0011] Preferably, in the above technical solution, the calcium carbonate is obtained by heating and drying the calcium carbonate at a temperature of 100-300° C. for 2-5 hours, and then grinding and sieving to obtain a material with a particle size of ≤60 mm.

[0012] Preferably, in the above technical solution, the powdered grinding aid is mainly made of the following raw materials in percentage by weight: 24-30% methyl dodecylaminopropionate, 6-12% montmorillonite, 6-11% nano silicon dioxide, 31-51% medium calcium fly ash, and 11-16% additives.

[0013] Preferably, in the above technical solution, the additives include polyacrylamide, boric acid, nano-calcium silicate and silane.

[0014] Preferably, in the above technical solution, the mass ratio of polyacrylamide, boric acid, nano-calcium silicate and silane in the additive is 5-15:5-15:4-9:4-9.

[0015] Preferably, in the above technical solution, the silane is methyltrimethoxysilane or hexadecyltrimethylsilane.

[0016] Preferably, in the above technical solution, the particle size of the montmorillonite is ≤10 mm.

[0017] Secondly, the present application provides a cement using the powdered cement grinding aid, which adopts the following technical solution:

[0018] A cement using the powdered cement grinding aid is prepared from the powdered cement grinding aid for promoting cement grinding.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The principle of adding medium-calcium fly ash to improve the cement grinding effect and increase the compressive strength of concrete is as follows: first, calcium carbonate and calcium chloride are added during the preparation of medium-calcium fly ash to promote the conversion of some substances in the fly ash into calcium feldspar, thereby increasing the hardness of the medium-calcium fly ash. During the cement grinding process, the friction between the cement material and the cement ball mill liner is enhanced, thereby improving the grinding effect. At the same time, calcium feldspar can be used as a cementing material to form a chemical precipitate that plays a bonding role between the concrete material particles, thereby improving the compressive strength of the concrete; secondly, the particle size of the medium-calcium fly ash is limited during the cement grinding process. In the process, under the synergistic effect of polyacrylamide, medium-calcium fly ash stably adheres to the surface of cement materials, enhances the friction of cement materials during grinding, and promotes cement grinding. At the same time, the MgO hydration products of medium-calcium fly ash, magnesium hydroxide crystals and SiO2 react with sodium hydroxide to form hydrated calcium silicate and calcium silicate, which fill the pores between concrete, improve the density of concrete, and thus improve the compressive strength of concrete; finally, the rough irregular particles on the surface of medium-calcium fly ash form tightly linked aggregates, which are evenly adhered to the cement materials, and the buildings made of this cement are evenly stressed. DETAILED DESCRIPTION

[0021] The specific implementation modes of the present invention are described in detail below in conjunction with specific embodiments, but it should be understood that the protection scope of the present invention is not limited by the specific implementation modes.

[0022] Example 1

[0023] A powdered cement grinding aid for promoting cement grinding, mainly made of the following raw materials: methyl dodecylaminopropionate, montmorillonite, nano silicon dioxide, medium calcium fly ash, and additives;

[0024] The additives include polyacrylamide, boric acid, nano calcium silicate and silane;

[0025] The preparation method of the medium-calcium fly ash is as follows: calcium carbonate, calcium chloride and fly ash are mixed evenly and then calcined for a period of time at a temperature of 1300-1500° C. to obtain the medium-calcium fly ash.

[0026] A cement prepared by using the powdered cement grinding aid for promoting cement grinding.

[0027] Example 2

[0028] A powdered cement grinding aid for promoting cement grinding, mainly made of the following raw materials: 24-30% of methyl dodecylaminopropionate, 8-12% of montmorillonite, 6-11% of nano silicon dioxide, 31-51% of medium calcium fly ash, and 11-16% of additives;

[0029] The additives include polyacrylamide, boric acid, nano calcium silicate and silane;

[0030] The preparation method of the medium-calcium fly ash is as follows: calcium carbonate, calcium chloride and fly ash are mixed and calcined at a temperature of 1300-1500° C. for 8 hours, and after calcination, the mixture is ground and sieved to obtain a material with a particle size of ≤8 mm.

[0031] A cement prepared by using the powdered cement grinding aid for promoting cement grinding.

[0032] Example 3

[0033] A powdered cement grinding aid for promoting cement grinding, mainly made of the following raw materials: 30% methyl dodecylaminopropionate, 11% nano silicon dioxide, 31% medium calcium fly ash, 16% additives, 12% montmorillonite, and the montmorillonite particle size is ≤10mm;

[0034] The additive is a mixture of polyacrylamide, boric acid, nano calcium silicate and methyltrimethoxysilane in a mass ratio of 5:5:4:4;

[0035] The preparation method of the medium calcium fly ash is as follows: 11.5% calcium carbonate, 0.1% calcium chloride and 88.4% fly ash are mixed and calcined at 1300° C. for 6 hours, and then ground and sieved to obtain a material with a particle size of ≤8 mm.

[0036] A cement prepared by using the powdered cement grinding aid for promoting cement grinding.

[0037] Example 4

[0038] A powdered cement grinding aid for promoting cement grinding, mainly made of the following raw materials: 27% methyl dodecylaminopropionate, 8% nano silicon dioxide, 44% medium calcium fly ash, 13% additives, 8% montmorillonite, and the montmorillonite particle size is 10 mm;

[0039] The additive is a mixture of polyacrylamide, boric acid, nano calcium silicate and hexadecyltrimethylsilane in a mass ratio of 15:15:9:8;

[0040] The preparation method of the medium-calcium fly ash is as follows: first, calcium carbonate is heated and dried at a temperature of 100° C. for 5 hours, and then ground and sieved to obtain calcium carbonate with a particle size of 60 mm; 11.5% calcium carbonate, 0.5% calcium chloride and 88% fly ash are mixed and calcined at a temperature of 1500° C. for 8 hours; after calcination, the mixture is ground and sieved to obtain a material with a particle size of 8 mm.

[0041] A cement prepared by using the powdered cement grinding aid for promoting cement grinding.

[0042] Example 5

[0043] A powdered cement grinding aid for promoting cement grinding, mainly made of the following raw materials: 24% methyl dodecylaminopropionate, 6% nano silicon dioxide, 51% medium calcium fly ash, 11% additives, 8% montmorillonite, and the montmorillonite particle size is 5mm;

[0044] The additive is a mixture of polyacrylamide, boric acid, nano calcium silicate, hexadecyltrimethylsilane and methyltrimethoxysilane in a mass ratio of 10:10:6:3:3;

[0045] The preparation method of the medium-calcium fly ash is as follows: first, calcium carbonate is heated and dried at 300° C. for 2 hours, and then ground and sieved to obtain calcium carbonate with a particle size of 30 mm; 19.4% calcium carbonate, 0.1% calcium chloride and 80.5% fly ash are mixed and calcined at 1300° C. for 7 hours; after calcination, the mixture is ground and sieved to obtain a material with a particle size of 4 mm.

[0046] A cement prepared by using the powdered cement grinding aid for promoting cement grinding.

[0047] Example 6

[0048] A powdered cement grinding aid for promoting cement grinding, mainly made of the following raw materials: 28% methyl dodecylaminopropionate, 11% nano silicon dioxide, 35% medium calcium fly ash, 16% additives, 10% montmorillonite, and the montmorillonite particle size is ≤10mm;

[0049] The additive refers to polyacrylamide, boric acid, nano calcium silicate, hexadecyltrimethylsilane and methyltrimethoxysilane mixed in a mass ratio of 9:8:9:5:4;

[0050] The preparation method of the medium-calcium fly ash is as follows: first, calcium carbonate is heated and dried at a temperature of 200° C. for 3.5 hours, and then ground and sieved to obtain calcium carbonate with a particle size of ≤60 mm; 16.7% calcium carbonate, 0.3% calcium chloride and 83% fly ash are mixed and calcined at a temperature of 1400° C. for 7 hours; after calcination, the mixture is ground and sieved to obtain a material with a particle size of ≤8 mm.

[0051] A cement prepared by using the powdered cement grinding aid for promoting cement grinding.

[0052] Comparative Example 1

[0053] The method is basically the same as Example 6, except that the fly ash in the raw material is prepared by a different method. A powdered cement grinding aid for promoting cement grinding is mainly made of the following raw materials: 28% methyl dodecylaminopropionate, 11% nano silicon dioxide, 35% medium calcium fly ash, 16% additives, and 10% montmorillonite, and the montmorillonite particle size is ≤10 mm;

[0054] The additive refers to polyacrylamide, boric acid, nano calcium silicate, hexadecyltrimethylsilane and methyltrimethoxysilane mixed in a mass ratio of 9:8:9:5:4;

[0055] The fly ash preparation method is as follows: firstly, 0.5% sodium chloride, 80.1% fly ash and 19.4% sodium carbonate are uniformly mixed, roasted at 600° C. for 3 hours, ground and sieved, and then ground and sieved after calcination to obtain a material with a particle size of ≤8 mm.

[0056] Comparative Example 2

[0057] The invention is basically the same as Example 6, except that the raw material composition is different. A powdered cement grinding aid for promoting cement grinding is mainly made of the following raw materials: 47% methyl dodecylaminopropionate, 27% nano silicon dioxide, 15% additives, 11% montmorillonite, and the montmorillonite particle size is ≤10 mm;

[0058] The additive refers to polyacrylamide, boric acid, nano calcium silicate, hexadecyltrimethylsilane and methyltrimethoxysilane mixed in a mass ratio of 9:8:9:5:4;

[0059] A cement prepared by using the powdered cement grinding aid for promoting cement grinding.

[0060] Comparative Example 3

[0061] The invention is basically the same as Example 6, except that the composition of the additive raw materials is different. A powdered cement grinding aid for promoting cement grinding is mainly made of the following raw materials: 28% methyl dodecylaminopropionate, 11% nano silicon dioxide, 35% medium calcium fly ash, 16% additives, 10% montmorillonite, and the montmorillonite particle size is ≤10 mm;

[0062] The mass ratio of nano calcium silicate, hexadecyltrimethylsilane and methyltrimethoxysilane in the additive is 9:5:4;

[0063] The preparation method of the medium-calcium fly ash is as follows: first, calcium carbonate is heated and dried at 200° C. for 3.5 hours, then the calcium carbonate is ground and sieved, 16.7% calcium carbonate, 0.3% calcium chloride and 83% fly ash are mixed and calcined at 1400° C. for 7 hours, and then ground and sieved after calcination to obtain a material with a particle size of ≤8 mm.

[0064] A cement prepared by using the powdered cement grinding aid for promoting cement grinding.

[0065] Comparative Example 4

[0066] The basic composition is the same as that of embodiment 6, except that the raw material composition and additive ratio are different. A powdered cement grinding aid for promoting cement grinding is mainly made of the following raw materials: 53% medium calcium fly ash, 15% additives, 32% montmorillonite, and the montmorillonite particle size is ≤10mm;

[0067] The additive refers to polyacrylamide, boric acid, nano calcium silicate, hexadecyltrimethylsilane and methyltrimethoxysilane mixed in a mass ratio of 3:2:10:7:7;

[0068] The preparation method of the medium-calcium fly ash is as follows: first, calcium carbonate is heated and dried at a temperature of 200° C. for 3.5 hours, and then ground and sieved to obtain calcium carbonate with a particle size of ≤60 mm; 16.7% calcium carbonate, 0.3% calcium chloride and 83% fly ash are mixed and calcined at a temperature of 1400° C. for 7 hours; after calcination, the mixture is ground and sieved to obtain a material with a particle size of ≤8 mm.

[0069] A cement prepared by using the powdered cement grinding aid for promoting cement grinding.

[0070] Comparative Example 5

[0071] The invention is basically the same as Example 6, except that the additive components are different. A powdered cement grinding aid for promoting cement grinding is mainly made of the following raw materials: 37% methyl dodecylaminopropionate, 8% nano silicon dioxide, 32% medium calcium fly ash, 15% additives, 9% montmorillonite, and the montmorillonite particle size is ≤10 mm;

[0072] The mass ratio of polyacrylamide and boric acid in the additive is 9:8;

[0073] The preparation method of the medium-calcium fly ash is as follows: first, calcium carbonate is heated and dried at a temperature of 200° C. for 3.5 hours, and then ground and sieved to obtain calcium carbonate with a particle size of ≤60 mm; 16.7% calcium carbonate, 0.3% calcium chloride and 83% fly ash are mixed and calcined at a temperature of 1400° C. for 7 hours; after calcination, the mixture is ground and sieved to obtain a material with a particle size of ≤8 mm.

[0074] A cement prepared by using the powdered cement grinding aid for promoting cement grinding.

[0075] The compressive strength test of the cement using cement grinding aid obtained in Examples 1-6 and Comparative Examples 1-5 was conducted: 0.3% cement grinding aid was added to the cement raw material for grinding, the cement obtained after grinding was mixed with water, poured into a mold after mixing, and steam cured to obtain cement products, and then the prepared cement products were cured for 7 days, 14 days, and 28 days to test their compressive strength, and the test was conducted according to the method specified in GB / T17671-1999. The results are shown in Table 1.

[0076] Table 1 Compressive strength test results of cement using cement grinding aid

[0077]

[0078]

[0079] As shown in Table 1 above, the test results of Examples 4-6 are significantly better than those of Examples 1-3, indicating that Examples 4-6 limit the components and component ratios of the cement grinding aid, as well as the raw material preparation, and the cement prepared with the obtained cement grinding aid has good compressive strength and crack resistance on the 7th, 14th and 28th days. The test results of Example 6 are significantly better than those of Comparative Examples 1-5, indicating that the cement prepared with the cement grinding aid obtained in Example 6 of the method of the present invention has good compressive strength and crack resistance on the 7th, 14th and 28th days.

[0080] The anti-cracking performance of cement obtained by Examples 1-6 and Comparative Examples 1-5 using cement grinding aids was tested: the cement sample blocks were placed in an environment with a humidity of 90% and an ambient temperature of 25°C for curing, and the sample blocks were tested every 12 days to see if cracks were generated. The anti-cracking performance was: no cracks > cracks > cracks > obvious cracks. The results are shown in Table 2.

[0081] Table 2 Test results of anti-cracking performance of cement using cement grinding aid

[0082]

[0083]

[0084] The results are shown in Table 2. The crack resistance of Examples 3-6 is better than that of Examples 1-2, indicating that Examples 3-6 have better crack resistance. Compared with Comparative Examples 1-5, Example 6 using the method of the present invention shows that the cement prepared by the cement grinding aid obtained by the method of the present invention has better crack resistance.

[0085] The powdered cement grinding aids prepared by the method of Example 6 and Comparative Examples 1-5 and the commercially available grinding aids were added to the cement material and ground in a ball mill, and the additives in each formulation were tested. The test results are shown in Table 3. The unit of the output of each ball mill is tons / hour.

[0086] Table 3 Output and production rate of ball mill after adding various grinding agents

[0087]

[0088]

[0089] The results obtained in Table 3 show that the addition of the grinding aid obtained by the method of the present invention can significantly increase the output per hour of the ball mill. Compared with the blank test without adding the cement grinding aid, the production increase rate is 29.13%. Compared with comparative examples 1-5, the production increase rate is greater than 10%, indicating that the use of the method of the present invention is beneficial to improving the rate of grinding cement in the ball mill, thereby reducing the energy consumption of the ball mill and reducing the cost of cement grinding.

[0090] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.

Claims

1. A powdered cement grinding aid for promoting cement grinding, characterized in that: It is mainly made of the following raw materials: methyl dodecylaminopropionate, montmorillonite, nano silicon dioxide, medium calcium fly ash, additives; The preparation method of the medium-calcium fly ash is as follows: calcium carbonate, calcium chloride and fly ash are mixed evenly and then calcined for a period of time at a temperature of 1300-1500° C. to obtain the medium-calcium fly ash.

2. The powdered cement grinding aid for promoting cement grinding according to claim 1, characterized in that: The preparation method of the medium calcium fly ash is as follows: calcium carbonate, calcium chloride and fly ash are mixed and calcined at a temperature of 1300-1500° C. for 6-8 hours, and after calcination, the mixture is ground and sieved to obtain a material with a particle size of ≤8 mm.

3. The method for preparing medium-calcium fly ash according to claim 2, characterized in that: Calculated by weight percentage, the ratio of raw materials required for the medium-calcium fly ash preparation method is: 11.5-19.4% calcium carbonate, 0.1-0.5% calcium chloride and 80-88.4% fly ash.

4. The method for preparing medium-calcium fly ash according to claim 3, characterized in that: The calcium carbonate is obtained by heating and drying the calcium carbonate at a temperature of 100-300° C. for 2-5 hours, and then grinding and sieving to obtain a material with a particle size of ≤60 mm.

5. The powdered cement grinding aid for promoting cement grinding according to claim 1, characterized in that: The powdered grinding aid is mainly made of the following raw materials in terms of weight percentage: 24-30% of methyl dodecylaminopropionate, 8-12% of montmorillonite, 6-11% of nano silicon dioxide, 31-51% of medium calcium fly ash, and 11-16% of additives.

6. The powdered cement grinding aid for promoting cement grinding according to claim 5, characterized in that: The additives include polyacrylamide, boric acid, nano calcium silicate and silane.

7. The powdered cement grinding aid for promoting cement grinding according to claim 6, characterized in that: The mass ratio of polyacrylamide, boric acid, nano calcium silicate and silane in the additive is 5-15:5-15:4-9:4-9.

8. The powdered cement grinding aid for promoting cement grinding according to claim 7, characterized in that: The silane includes one or both of methyltrimethoxysilane and hexadecyltrimethylsilane.

9. The powdered cement grinding aid for promoting cement grinding according to claim 5, characterized in that: The particle size of the montmorillonite is ≤10 mm.

10. A cement using the powdered cement grinding aid, characterized in that: The powdered cement grinding aid for promoting cement grinding is prepared using any one of claims 1 to 9.