High-mobility indium oxide-based target material as well as preparation method and application thereof
By using a variety of oxide doping additives in In2O3-based targets, the preparation of high-density indium oxide-based targets is achieved at low temperatures, the problems of taking into account both carrier mobility and light transmittance are solved, and TCO is improved The performance of the film is suitable for improving the photoelectric conversion efficiency of HJT batteries.
Patent Information
- Application Number
- CN202410907793.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-08
AI Technical Summary
When the existing In2O3-based targets are prepared at high sintering temperature, carrier mobility and light transmittance are difficult to take into account, and the increase in doping will reduce mobility and affect light transmittance, and the lack of low-temperature sintering and dense technology plan.
A variety of oxide doping additives, such as Y2O3, Dy2O3, Gd2O3, B2O3, Bi2O3, Ta2O5, MoO3 and WO3, are used to prepare high density by eutectic and liquid-phase filling technology at low doping and sintering temperature. Low grain size indium oxide-based targets for the preparation of TCO films with high light transmittance and high carrier mobility.
It realizes the preparation of high-density indium oxide-based targets at lower temperatures, improves the carrier mobility and light transmittance of TCO films, reduces production costs and energy consumption, and is suitable for improving the photoelectric conversion efficiency of HJT batteries.
Smart Images

Figure BDA0004932651180000101 
Figure BDA0004932651180000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of target materials for photovoltaic cells, and in particular to a high-mobility indium oxide-based target material and a preparation method and application thereof. Background Art
[0002] Silicon heterojunction solar cells (HJT cells) have high theoretical efficiency, simple preparation process and large cost reduction space. They are currently a hot research topic in the field of solar cells and one of the solar cells for large-scale industrialization. Transparent conductive oxide films (TCO films) have excellent conductivity and high transmittance. They are the core materials of HJT cells and an important guarantee for high photoelectric conversion efficiency.
[0003] At present, TCO films used in HJT batteries are mainly produced by magnetron sputtering coating of In2O3-based targets. The In2O3 content in this type of target is mostly 90-99wt%. By adjusting the type and content of doping elements, TCO films with different photoelectric properties can be obtained. With the development of the HJT battery industry, higher technical indicators have been proposed for the carrier mobility and transmittance of TCO films to enable HJT batteries to achieve higher conversion efficiency. The carrier mobility of TCO films prepared with pure In2O3 targets can reach 150cm 2 / V·S, which is much higher than the currently commercial TCO film. However, the high melting point of In2O3 (2000℃) makes the sintering temperature of its target material higher than 1800℃, which greatly increases energy consumption, production costs and equipment requirements. Traditional In2O3-based targets are usually doped with SnO2 to assist sintering to reduce the sintering temperature and increase the carrier concentration, but the sintering effect of SnO2 is general, and a higher doping amount can achieve a better sintering effect. However, in TCO films, the mobility is affected by the scattering between electrons and doped ions. The increase in the doping amount will increase the scattering during the movement of carriers, significantly reduce the carrier mobility of TCO films, and also have an adverse effect on its transmittance. At present, there is still a lack of technical solutions for low-doped In2O3-based targets with high carrier mobility and high transmittance, and which can be sintered densely at a lower temperature (≤1600℃).
[0004] Therefore, it is urgent to develop an In2O3-based target material with high mobility, high transmittance, low doping, and dense sintering at a relatively low temperature, while solving the problem of the difficulty in uniformly and efficiently incorporating low-doped oxides into the matrix, so as to further improve the performance of TCO films and HJT batteries, and expand the application scope and prospects of TCO films. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides an indium oxide-based target material. The indium oxide-based target material of the present invention has a low sintering temperature and a high density. The present invention achieves a target material with high density and low grain size at a low doping amount and sintering temperature by doping with a variety of oxides. The TCO film obtained by coating the indium oxide-based target material has a high transmittance and a high carrier mobility, which improves the performance of the TCO film and can be used in HJT cells to further improve the photoelectric conversion efficiency.
[0006] The invention also provides a method for preparing an indium oxide-based target material.
[0007] The invention also provides a TCO film.
[0008] The invention also provides a method for preparing a TCO film.
[0009] The invention also provides application of the indium oxide-based target material.
[0010] In a first aspect of the present invention, an indium oxide-based target material is provided, wherein the raw materials for preparation include indium oxide, X oxide, Y oxide and Z oxide;
[0011] Wherein, the X oxide includes at least one of Y2O3, Dy2O3 and Gd2O3;
[0012] The Y oxide includes at least one of B2O3 and Bi2O3;
[0013] The Z oxide includes at least one of Ta2O5, MoO3 and WO3.
[0014] According to a specific embodiment of the present invention, the indium oxide-based target material provided by the present invention has at least the following beneficial effects:
[0015] The maximum sintering temperature of the indium oxide-based target material of the present invention does not exceed 1600° C., which can reduce energy consumption, production cost and equipment requirements, and is more suitable for industrial large-scale production. The density of the indium oxide-based target material prepared by the present invention reaches more than 98.5%, and the average grain size range of the target material is 6.3-8.5 μm. The present invention obtains a target material with high density and low grain size by doping a variety of oxide additives. The TCO film obtained by coating the indium oxide-based target material prepared by the scheme of the present invention has excellent performance, and a high carrier mobility of 60 cm-1 is obtained while maintaining a relatively low carrier concentration. 2 / V·S or above, and the transmittance between wavelengths of 400 to 1200nm is more than 89%, which can be used in HJT cells to further improve the photoelectric conversion efficiency.
[0016] According to some embodiments of the present invention, the X oxide includes at least two of Y2O3, Dy2O3 and Gd2O3.
[0017] According to some embodiments of the present invention, the X oxide includes Y2O3, Dy2O3 and Gd2O3.
[0018] According to some embodiments of the present invention, the Y oxide includes B2O3 and Bi2O3.
[0019] The present invention uses X oxide and Z oxide as doping aids, and utilizes the higher than In 3+ Radius of rare earth metal ions Y 3+ 、Dy 3+ and Gd 3+ , and the small radius high valence element Ta in the Z oxide doping aid 5+ 、Mo 6+ and W 6+ Co-doping can effectively improve the doping efficiency and the crystal stability after doping, ensuring that the scattering centers of impurities are reduced with less doping amount, thereby improving the mobility of carriers.
[0020] Specifically, X oxide has higher doping activity. When doped into indium oxide, the lattice is distorted, defects increase, and the unit cell volume increases, making it easier for high-valent ions with smaller radius in Z oxide to enter the indium oxide lattice and replace indium ions, thereby improving the doping efficiency. Two different types of doped oxides occupy different In crystallographic positions in the unit cell, making the doping more symmetrical. The two have opposite effects on the unit cell volume, resulting in a smaller change in the overall unit cell volume. The combined effect of the two results in a smaller unit cell volume strain after doping, thereby improving the stability of the crystal after doping.
[0021] In the cubic In2O3 unit cell, there are two crystallographic positions for In, namely the 8b position and the 24d position. The In atom at the 8b position has exactly the same bond length as the six surrounding O atoms, and is missing two oxygen atoms on its body diagonal, while the In atom at the 24d position has a different bond length from the six surrounding O atoms, and its missing oxygen is distributed on the face diagonal. 3+ The radius is 0.094nm, but the radius of high-valent ions (≥+5) is often less than 0.08nm, such as Ta 5+ 、Mo 6+ , W 6+ The radii are 0.078nm, 0.073nm, and 0.074nm respectively; this is similar to In 3+ The radius is quite different, so the efficiency of high-valent ions doped alone is low. Therefore, the present invention further optimizes the doping scheme of low-doped indium oxide, and selects a doping active ion with a radius larger than In. 3+ Rare earth ions Y with small radius difference3+ (0.104nm), Dy 3+ (0.105nm), Gd 3+ (0.108nm) co-doping can improve doping efficiency and crystal stability, improve target quality, and further improve the mobility and transmittance of TCO films prepared from the target.
[0022] The present invention also found that when the three X oxides Y2O3, Dy2O3 and Gd2O3 are all doped, the comprehensive performance of the prepared target material and TCO film is the best, and all performance data are good. The reasonable ratio of the three X oxides achieves a relatively better technical effect, which may be related to the special distribution of extranuclear electrons of rare earth ions.
[0023] In addition, the X oxide doping aid used in the present invention can also be used as a solid-phase sintering aid, which can appropriately reduce the sintering temperature by reducing the sintering activation energy. It destroys the stability of the crystal structure of the indium oxide matrix material, produces lattice distortion or defects, thereby promoting mass transfer, promoting densification and helping to improve doping efficiency.
[0024] The present invention uses Y oxide doping aid as a liquid phase sintering aid, which eutectics with the indium oxide matrix material at a relatively low temperature to form a liquid phase, and achieves the purpose of sintering and densification at a relatively low temperature through the flow of the liquid phase to fill pores and the "dissolution-precipitation" effect. The present invention uses two sintering aids in combination to achieve the technical effect of optimally reducing the maximum sintering temperature and promoting the densification of the target material.
[0025] According to some embodiments of the present invention, the indium oxide, the X oxide, the Y oxide and the Z oxide are all powders.
[0026] According to some embodiments of the present invention, the median particle size of the indium oxide powder is in the range of 0.31 μm < D 50 <0.45μm, the median particle size range of the X oxide powder is 1.26μm<D 50 <1.75μm, the median particle size range of the Y oxide powder is 2.15μm<D 50 <3.36μm, the median particle size of the Z oxide powder is 1.86μm<D 50 <3.15μm.
[0027] According to some embodiments of the present invention, the preparation raw materials include, by mass, 98.1-99.6 parts of indium oxide, 0.05-0.7 parts of X oxide, 0.05-0.7 parts of Y oxide and 0.05-0.6 parts of Z oxide.
[0028] According to some embodiments of the present invention, the preparation raw materials include, by mass, 98.5-99.5 parts of indium oxide, 0.2-0.6 parts of X oxide, 0.2-0.4 parts of Y oxide and 0.1-0.5 parts of Z oxide.
[0029] According to some embodiments of the present invention, the preparation raw materials include, by mass, 98.8-99.5 parts of indium oxide, 0.3-0.5 parts of X oxide, 0.2-0.4 parts of Y oxide and 0.2-0.5 parts of Z oxide.
[0030] According to some embodiments of the present invention, the preparation raw materials further include a dispersant, a binder, a plasticizer and water.
[0031] According to some embodiments of the present invention, the preparation raw materials further include 0.2 to 1 parts of a dispersant, 0.1 to 0.3 parts of a binder, 0.5 to 2 parts of a plasticizer and 100 to 200 parts of water.
[0032] According to some embodiments of the invention, the dispersant is polyvinyl pyrrolidone.
[0033] The present invention helps to improve the uniformity of mixing various oxide doping aids with the indium oxide matrix by using a dispersant during the preparation process of the indium oxide-based target material, thereby helping to improve the doping activity.
[0034] According to some embodiments of the present invention, the binder includes at least one of polyvinyl alcohol, polyethylene oxide, and polyvinylidene fluoride.
[0035] According to some embodiments of the invention, the plasticizer is polyethylene glycol.
[0036] The second aspect of the present invention provides a method for preparing the indium oxide-based target material according to the first aspect of the present invention, comprising the following steps:
[0037] S1, mixing X, Y and Z oxides, dispersing and grinding, adding indium oxide and grinding, and granulating to obtain a mixed powder;
[0038] S2. Cold isostatic pressing, degreasing and sintering to obtain the indium oxide-based target material.
[0039] According to some embodiments of the present invention, in step S1, a dispersant and water are added before dispersion and grinding to obtain slurry 1 by dispersion and grinding; and indium oxide is added and ground to obtain slurry 2 by step S1.
[0040] According to some embodiments of the present invention, the median particle size of the slurry 1 is controlled to be D 50 ≤0.2μm.
[0041] According to some embodiments of the present invention, the median particle size of the slurry 2 is controlled to be D50 ≤0.13μm.
[0042] The present invention improves the doping uniformity and doping efficiency of the doped oxide additive through a two-step mixing scheme. Combined with the improvement of the conventional process by the scheme of the present invention, firstly, low-content doped oxides X, Y and Z are mixed and ball-milled in advance to obtain slurry 1, and the particle size of the powder is controlled to be smaller than that of the indium oxide powder by grinding, and then the doped oxide powder is mixed with the indium oxide powder to make the mixing more complete, achieve a better sintering effect, and make the target material elements more evenly distributed, which can effectively improve the doping activity of the doped oxide, thereby making the film prepared by magnetron sputtering more uniform and having better performance. The present invention further improves the target material and TCO film performance by more than 10% through the improvement of the preparation process.
[0043] According to some embodiments of the invention, the grinding is ball milling.
[0044] According to some embodiments of the present invention, the sintering in step S2 includes three stages;
[0045] Among them, the sintering temperature in the first stage is 600-800°C, and the holding time is 1-5h;
[0046] The second stage sintering temperature is 900-980℃, and the holding time is 3-8h;
[0047] The third stage is sintering in an oxygen atmosphere, the sintering temperature is 1450-1600°C, and the holding time is 5-12h.
[0048] Preferably, the third stage sintering temperature is 1450-1550°C.
[0049] In a third aspect of the present invention, there is provided a TCO film prepared using the indium oxide-based target material according to the first aspect of the present invention, wherein the carrier concentration of the TCO film is 1.2×10 20 ~2.8×10 20 cm -3 , mobility ≥ 60cm 2 / V·S, the transmittance between wavelengths of 400 and 1200 nm is ≥89%.
[0050] According to some embodiments of the present invention, the carrier concentration of the TCO film is 1.58×10 20 ~2.65×10 20 cm -3 , mobility ≥ 66.8cm 2 / V·S, the transmittance between wavelengths of 400 and 1200 nm is ≥89.6%.
[0051] A fourth aspect of the present invention provides a method for preparing a TCO film as described in the third aspect of the present invention, comprising the following steps:
[0052] The target material described in the first aspect of the present invention is used to form a TCO film by magnetron sputtering with a coating power of 1-10 kW and a coating thickness of 20-200 nm.
[0053] According to some embodiments of the present invention, the coating power is 3-8 kW, and the coating thickness is 60-120 nm.
[0054] According to some embodiments of the present invention, the method for preparing the TCO thin film further comprises an annealing step after coating, wherein the annealing step is annealing in a muffle furnace at a temperature of 150° C. to 250° C. for 20 to 40 minutes.
[0055] The fifth aspect of the present invention provides the application of the target material described in the first aspect of the present invention, or the preparation method described in the second aspect of the present invention, or the TCO film described in the third aspect of the present invention, or the preparation method described in the fourth aspect of the present invention in the field of HJT batteries.
[0056] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be obvious from the description, or may be learned by practice of the present invention. DETAILED DESCRIPTION
[0057] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0058] If the specific conditions are not specified in the specific implementation mode, the conventional conditions or the conditions recommended by the manufacturer are used. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased from the market.
[0059] Example 1
[0060] This embodiment provides a high-mobility, low-doped indium oxide-based target material and a preparation method thereof.
[0061] The raw materials of the indium oxide-based target material of this embodiment are calculated by mass as follows: 99 parts of In2O3, 0.1 parts of X oxide: 0.1 parts of Dy2O3, 0.3 parts of Y2O3 and 0.1 parts of Gd2O3, 0.2 parts of Y oxide: 0.1 parts of B2O3 and 0.1 parts of Bi2O3, and 0.2 parts of Z oxide: Ta2O5;
[0062] Among them, all raw materials are oxide powders with a purity of more than 4N; the median particle size range of In2O3 powder is 0.31μm<D 50 <0.45μm, the median particle size range of X powder is 1.26μm<D 50 <1.75μm, the median particle size of Y powder is 2.15μm<D 50 <3.36μm, the median particle size of Z powder is 1.86μm<D 50 <3.15μm.
[0063] The specific steps of the method for preparing the indium oxide-based target material of this embodiment are as follows:
[0064] 1) Ball milling, mixing and granulation of powder:
[0065] The X, Y and Z powders were mixed, 1.5 parts of deionized water and 0.005 parts of dispersant polyvinyl pyrrolidone (PVP) were added, and the mixed slurry 1 was obtained by ball milling with a sand mill. The ball milling time was 6 hours. The median particle size D of the mixed powder of slurry 1 was 50 ≤0.20μm;
[0066] In2O3 powder, 148.5 parts of ionized water and 0.495 parts of PVP were added to slurry 1. Slurry 2 was obtained by ball milling with a sand mill for 7 hours. The median particle size D 50 ≤0.13μm;
[0067] On the basis of slurry 2, 0.16 parts of a binder (PVA) and 0.8 parts of a plasticizer (PEG) were added, mixed and spray granulated to obtain granulated powder.
[0068] 2) Green billet forming:
[0069] The granulated powder was injected into the mold using a rotating target mold, and then packaged and placed in the chamber of a hydraulic press. The molding pressure was 185 MPa, and the rotating target blank was obtained by demolding after cold isostatic pressing.
[0070] 3) Debinding and sintering:
[0071] After the target blank is degreased, it is sintered in a sintering furnace: the first stage sintering temperature is 700℃, the holding time is 3h, the second stage sintering temperature is 940℃, the holding time is 5.5h, and the third stage uses the highest temperature sintering, the sintering temperature is 1520℃, oxygen is introduced, the oxygen introduction rate is 42.5L / min, and the pressure is 2.35kg / cm 2 , and kept warm for 8.5 hours in an oxygen atmosphere; a dense indium oxide-based target was obtained.
[0072] This embodiment further provides a method for flaw detection and coating of the prepared indium oxide-based target material, and the specific method is as follows:
[0073] Binding flaw detection: The prepared rotating target coated with indium is bound to the titanium tube and ultrasonic flaw detection is used, and no dark cracks are found.
[0074] TCO thin film coating: On the cleaned glass substrate, TCO thin film was deposited by magnetron sputtering with a coating power of 3 kW and a deposited film thickness of 90 nm. Then, it was annealed in a muffle furnace at 200°C in an air atmosphere for 30 min to obtain a TCO thin film, which was then subjected to performance testing.
[0075] Example 2
[0076] This embodiment provides a high-mobility, low-doped indium oxide-based target material and a preparation method thereof.
[0077] The difference between this embodiment and embodiment 1 is that in this embodiment, Z oxide is replaced by an equal amount of MoO3, and the highest sintering temperature in the third stage of the sintering step is 1480°C; other raw materials and preparation methods of this embodiment are the same as those of embodiment 1.
[0078] Example 3
[0079] This embodiment provides a high-mobility, low-doped indium oxide-based target material and a preparation method thereof.
[0080] The difference between this embodiment and embodiment 1 is that in this embodiment, Z oxide is replaced by an equal amount of WO3, and the highest sintering temperature in the third stage of the sintering step is 1500°C; other raw materials and preparation methods of this embodiment are the same as those of embodiment 1.
[0081] Example 4
[0082] This embodiment provides a high-mobility, low-doped indium oxide-based target material and a preparation method thereof.
[0083] The difference between this embodiment and embodiment 1 is that in this embodiment, X oxide is replaced by 0.5 parts of Y2O3, and the highest sintering temperature in the third stage of the sintering step is 1550°C; other raw materials and preparation methods of this embodiment are the same as those of embodiment 1.
[0084] Example 5
[0085] This embodiment provides a high-mobility, low-doped indium oxide-based target material and a preparation method thereof.
[0086] The difference between this embodiment and embodiment 4 is that in this embodiment, Z oxide is replaced by an equal amount of MoO3, and the highest sintering temperature in the third stage of the sintering step is 1500°C; the other raw materials and preparation method of this embodiment are the same as those of embodiment 4.
[0087] Example 6
[0088] This embodiment provides a high-mobility, low-doped indium oxide-based target material and a preparation method thereof.
[0089] The difference between this embodiment and embodiment 4 is that in this embodiment, Z oxide is replaced by an equal amount of WO3, and the highest sintering temperature in the third stage of the sintering step is 1530°C; other raw materials and preparation methods of this embodiment are the same as those of embodiment 4.
[0090] Example 7
[0091] This embodiment provides a high-mobility, low-doped indium oxide-based target material and a preparation method thereof.
[0092] The raw materials of the indium oxide-based target material of this embodiment are, by mass, 99 parts of In2O3, 0.2 parts of X oxide: Dy2O3 and 0.3 parts of Y2O3, 0.2 parts of Y oxide: B2O3, 0.3 parts of Z oxide: Ta2O5, and the highest sintering temperature in the third stage of the sintering step is 1520°C; the other preparation methods are the same as those in Example 1.
[0093] Example 8
[0094] This embodiment provides a high-mobility, low-doped indium oxide-based target material and a preparation method thereof.
[0095] The raw materials of the indium oxide-based target material of this embodiment are, by mass, 99 parts of In2O3, 0.2 parts of X oxide: Dy2O3 and 0.3 parts of Y2O3, 0.2 parts of Y oxide: Bi2O3, 0.3 parts of Z oxide: Ta2O5, and the highest sintering temperature in the third stage of the sintering step is 1550°C; the other preparation methods are the same as those in Example 1.
[0096] Example 9
[0097] This embodiment provides a high-mobility, low-doped indium oxide-based target material and a preparation method thereof.
[0098] The raw materials of the indium oxide-based target material of this embodiment are, by mass, 99 parts of In2O3, 0.1 parts of X oxide: Dy2O3 and 0.3 parts of Gd2O3, 0.3 parts of Y oxide: B2O3, 0.3 parts of Z oxide: MoO3, and the highest sintering temperature in the third stage of the sintering step is 1500°C; the other preparation methods are the same as those in Example 1.
[0099] Example 10
[0100] This embodiment provides a high-mobility, low-doped indium oxide-based target material and a preparation method thereof.
[0101] The raw materials of the indium oxide-based target material of this embodiment are, by mass, 99 parts of In2O3, 0.3 parts of X oxide: Gd2O3, 0.2 parts of Y oxide: Bi2O3, and 0.5 parts of Z oxide: MoO3. The highest sintering temperature in the third stage of the sintering step is 1480°C. The other preparation methods are the same as those in Example 1.
[0102] Comparative Example 1
[0103] This comparative example provides an indium oxide-based target material and a preparation method thereof.
[0104] The raw materials of the indium oxide-based target material of this comparative example are, by mass, 99 parts of In2O3 and 1 part of SnO2;
[0105] Among them, all raw materials are oxide powders with a purity of more than 4N; the median particle size range of In2O3 powder is 0.31μm<D 50 <0.45μm, the median particle size of SnO2 powder is 1.86μm<D 50 <3.15μm.
[0106] The specific steps of the preparation method of the indium oxide-based target material of this comparative example are as follows:
[0107] 1) Ball milling, mixing and granulation of powder:
[0108] Deionized water and dispersant polyvinyl pyrrolidone (PVP) were added to the SnO2 powder, and the slurry 1 was obtained by ball milling with a sand mill. The ball milling time was 6 h. The median particle size D 50 ≤0.20μm;
[0109] In2O3 powder and deionized water were added to slurry 1, and slurry 2 was obtained by ball milling with a sand mill. The ball milling time was 7 hours. The median particle size D 50 ≤0.13μm;
[0110] On the basis of slurry 2, 0.16 parts of a binder (PVA) and 0.8 parts of a plasticizer (PEG) were added, mixed and spray granulated to obtain granulated powder.
[0111] 2) Green billet forming:
[0112] The granulated powder was injected into the mold using a rotating target mold, and then packaged and placed in the chamber of a hydraulic press. The molding pressure was 185 MPa, and the rotating target blank was obtained by demolding after cold isostatic pressing.
[0113] 3) Debinding and sintering:
[0114] After degreasing the target blank, it is sintered in a sintering furnace: the sintering temperature in the first stage is 70°C, and the holding time is 3 hours; the sintering temperature in the second stage is 940°C, and the holding time is 5.5 hours; the third stage uses the highest sintering temperature, the sintering temperature is 1650°C, oxygen is introduced, and the temperature is kept for 8.5 hours in an oxygen atmosphere; a dense indium oxide-based target is obtained.
[0115] This comparative example further provides a method for flaw detection and coating of the prepared indium oxide-based target material, and the specific method is as follows:
[0116] Binding flaw detection: The prepared rotating target coated with indium is bound to the titanium tube and ultrasonic flaw detection is used, and no dark cracks are found.
[0117] TCO thin film coating: On the cleaned glass substrate, TCO thin film was deposited by magnetron sputtering with a coating power of 3 kW and a deposited film thickness of 90 nm. Then, it was annealed in a muffle furnace at 200°C in an air atmosphere for 30 min to obtain a TCO thin film, which was then subjected to performance testing.
[0118] Comparative Example 2
[0119] This comparative example provides an indium oxide-based target material and a preparation method thereof.
[0120] The raw materials of the indium oxide-based target material of this comparative example are 97 parts of In2O3 and 3 parts of SnO2 by mass. The highest sintering temperature in the third stage of the sintering step is 1600°C. The other preparation methods are the same as those of comparative example 1.
[0121] Comparative Example 3
[0122] This comparative example provides an indium oxide-based target material and a preparation method thereof.
[0123] The raw materials of the indium oxide-based target material of this comparative example are 90 parts by mass of In2O3 and 10 parts by mass of SnO2. The highest sintering temperature in the third stage of the sintering step is 1550°C. The other preparation methods are the same as those of Comparative Example 1.
[0124] Comparative Example 4
[0125] This comparative example provides an indium oxide-based target material and a preparation method thereof.
[0126] The raw materials for preparation of this comparative example are the same as those in Example 3. The difference between this comparative example and Example 3 is that in the preparation method of this comparative example, in the ball milling, mixing and granulation steps of the powder, each raw material is mixed with deionized water and a dispersant once and then ball milled in a sand mill to obtain a slurry. The ball milling time is 7 hours, and the median particle size D of the slurry is 50≤0.13 μm, the highest sintering temperature in the third stage of the sintering step is 1560°C; the other preparation steps are the same as those in Example 3.
[0127] Comparative Example 5
[0128] This comparative example provides an indium oxide-based target material and a preparation method thereof.
[0129] The raw materials of the indium oxide-based target material of this comparative example are, by mass, 99 parts of In2O3, 0.16 parts of X oxide Dy2O3, 0.48 parts of Y2O3, 0.16 parts of Gd2O3, and 0.2 parts of Z oxide MoO3. The highest sintering temperature in the third stage of the sintering step is 1620°C. The other preparation methods are the same as those in Example 1.
[0130] Comparative Example 6
[0131] This comparative example provides an indium oxide-based target material and a preparation method thereof.
[0132] The raw materials of the indium oxide-based target material of this comparative example are, by mass, 99 parts of In2O3, 0.53 parts of Y oxide: B2O3, 0.27 parts of Bi2O3, and 0.2 parts of Z oxide MoO3. The highest sintering temperature in the third stage of the sintering step is 1600°C. The other preparation methods are the same as those in Example 1.
[0133] Comparative Example 7
[0134] This comparative example provides an indium oxide-based target material and a preparation method thereof.
[0135] The raw materials of the indium oxide-based target material of this comparative example are, by mass, 99.2 parts of In2O3, 0.1 parts of X oxide: Dy2O3, 0.3 parts of Y2O3 and 0.1 parts of Gd2O3, 0.2 parts of Y oxide: B2O3 and 0.1 parts of Bi2O3, and the highest sintering temperature in the third stage of the sintering step is 1560°C; the other preparation methods are the same as those in Example 1.
[0136] The oxide raw material ratios of the embodiments and comparative examples of the present invention are shown in Table 1:
[0137] Table 1 Oxide raw material ratios of various embodiments and comparative examples
[0138]
[0139] Test example:
[0140] The density and average grain size of the target materials prepared in each embodiment and comparative example were tested, and the carrier mobility, carrier concentration and transmittance of the prepared TCO film were tested. Among them, the average grain size was measured by the intercept method; the target density was tested by the Archimedean drainage method; the carrier mobility and concentration of the film were tested by the Hall effect tester, and the transmittance of the film was tested by the UV-visible near-infrared spectrophotometer. The test results are shown in Table 2:
[0141] Table 2 Performance test data of target materials and TCO films prepared in various embodiments and comparative examples
[0142]
[0143] From the above test results, it can be seen that when the low-doped indium oxide-based target is prepared using the scheme of the present invention, the maximum sintering temperature range is 1480-1550°C, the density of the prepared indium oxide-based target reaches more than 98.5%, and the average grain size range of the target is 6.3-8.5μm. Therefore, the present invention achieves the acquisition of a high-density target with a low grain size at a low doping amount and sintering temperature by using a variety of doped oxides. The indium oxide-based target prepared by the scheme of the present invention is magnetron sputtered on glass to obtain a TCO film, and the carrier concentration of the film reaches 1.58×10 20 ~2.65×10 20 cm -3 , the carrier mobility reaches 66.8-85.1cm 2 / V·S, and the transmittance is 89.6% to 91.6%. The test results show that the TCO film prepared by the scheme of the present invention can obtain high transmittance and high carrier mobility while maintaining a low free carrier concentration, thereby achieving high performance of the TCO film and being used in HJT batteries to help improve their photoelectric conversion efficiency.
[0144] Comparative Examples 1 to 3 use conventional tin oxide doping, where the tin oxide doping amount of Comparative Example 1 is the same as that of Examples 1 to 10, but the sintering temperature of its target material is as high as 1650°C, and the target material density is only 95.3%, which is much lower than the target material prepared by the scheme of the present invention, indicating that the sintering aid effect of tin oxide is not as good as the composite oxide doping aid of the scheme of the present invention. In addition, the mobility and light transmittance of the TCO film prepared by the target material of Comparative Example 1 are also much lower than those of Examples 1 to 10. On the one hand, it may be that the poor density of its target material affects the coating quality, and on the other hand, it may be that tin oxide is doped in the indium oxide-based target material, which has a significant adverse effect on the conductivity and light transmittance of the indium oxide-based target material compared with the composite doping aid of the scheme of the present invention. In Comparative Examples 2 and 3, the doping amount of tin oxide is increased, so that the sintering temperature of the target material is reduced and the density is increased, but the carrier mobility of the TCO film prepared by the target material is reduced and the concentration is increased, resulting in a significant decrease in the performance of the TCO film. This is mainly because the increase in the doping amount increases the carrier concentration and the content of impurity scattering centers, thereby reducing the mobility.
[0145] The raw material ratio of Comparative Example 4 is the same as that of Example 3, but the sintering temperature of the target material of Comparative Example 4 is higher, and the various properties of the TCO film prepared therefrom are also worse than those of Example 3, indicating that the preparation scheme of Comparative Example 4 uses a one-time mixing scheme for each raw material, and the mixing uniformity of its low-doping component and the indium oxide matrix is lower than that of Example 3 using a secondary mixing scheme, resulting in lower doping efficiency, and then lower carrier concentration, and more impurities are precipitated at the grain boundaries, thereby reducing the mobility.
[0146] In Comparative Example 5, the Y oxide doping agent was omitted, resulting in a significantly higher sintering temperature than in Examples 1 to 10, reaching 1620°C, and the density of the target material prepared by it was also difficult to reach a high level. In Comparative Example 6, the X oxide doping agent was omitted, resulting in a higher sintering temperature than in Examples 1 to 10, and the carrier mobility and light transmittance of the TCO film prepared by it were significantly reduced, and the performance of the TCO film deteriorated.
[0147] In Comparative Example 7, Z oxide is missing, and the carrier concentration of the TCO film prepared therefrom is significantly lower than that of Examples 1 to 10, and the mobility is also lower than that of Examples 1 to 10, which will cause the conductivity of the film to drop sharply, making it difficult to meet the electrical performance requirements of the HJT battery for the TCO film. The reason is that on the one hand, the incorporation of high-valent oxide Z can increase the carrier concentration, and on the other hand, the radius of Z ions is small, which can reduce the lattice expansion caused by the incorporation of X oxide, thereby reducing the lattice distortion and helping to improve the carrier mobility.
[0148] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. An indium oxide-based target material, characterized in that: The preparation raw materials include indium oxide, X oxide, Y oxide and Z oxide; Wherein, the X oxide includes at least one of Y2O3, Dy2O3 and Gd2O3; The Y oxide includes at least one of B2O3 and Bi2O3; The Z oxide includes at least one of Ta2O5, MoO3 and WO3.
2. The indium oxide-based target material according to claim 1, characterized in that: The preparation raw materials include, by weight, 98.1 to 99.6 parts of indium oxide, 0.05 to 0.7 parts of X oxide, 0.05 to 0.7 parts of Y oxide and 0.05 to 0.6 parts of Z oxide.
3. The indium oxide-based target material according to claim 1, characterized in that: The preparation raw materials also include a dispersant, a binder, a plasticizer and water.
4. The indium oxide-based target material according to claim 1, characterized in that: The X oxides include Y2O3, Dy2O3 and Gd2O3.
5. The method for preparing an indium oxide-based target material according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1, mixing X, Y and Z oxides, dispersing and grinding, adding indium oxide and grinding, and granulating to obtain a mixed powder; S2. Cold isostatic pressing, degreasing and sintering to obtain the indium oxide-based target material.
6. The preparation method according to claim 5, characterized in that: In step S1, a dispersant and water are added before dispersion and grinding, and slurry 1 is obtained by dispersion and grinding. In step S1, indium oxide is added and ground to obtain slurry 2.
7. The preparation method according to claim 5, characterized in that: The sintering in step S2 includes three stages; Among them, the sintering temperature in the first stage is 600-800°C, and the holding time is 1-5h; The second stage sintering temperature is 900-980℃, and the holding time is 3-8h; The third stage is sintering in an oxygen atmosphere, the sintering temperature is 1450-1600°C, and the holding time is 5-12h.
8. A TCO film, characterized in that: The TCO film is prepared using the target material according to any one of claims 1 to 4; the carrier concentration of the TCO film is 1.2×10 20 ~2.8×10 20 cm -3 , mobility ≥ 60cm 2 / V·S, the transmittance between wavelengths of 400 and 1200 nm is ≥89%.
9. The method for preparing a TCO thin film according to claim 8, characterized in that: The following steps are involved: The target material according to any one of claims 1 to 4 is used for film coating by magnetron sputtering, with a coating power of 1 to 10 kW and a coating thickness of 20 to 200 nm to obtain a TCO film.
10. Use of the target material according to any one of claims 1 to 4, the preparation method according to any one of claims 5 to 7, the TCO film according to claim 8 or the preparation method according to claim 9 in the field of HJT batteries.
Citation Information
Patent Citations
Thin film transistor having crystalline indium oxide semiconductor film
CN102916052A
Indium tantalum yttrium oxide powder and preparation method thereof
CN114163217A
High-valence element doped indium tin oxide material as well as preparation method and application thereof
CN116730710A
Production of compound oxide sintered body
JP1999302074A
Sintered bodies and amorphous films
JP5550768B1
Cited By
Low-indium ceramic target material as well as preparation method and application thereof
CN120622917A
Low-indium ceramic target material, method for preparing same, and use thereof
CN120622917B
Low-indium RPD target material and preparation method and application thereof
CN121159245A
High-mobility indium-oxide-based target material, and preparation method therefor and use thereof
WO2026011687A1