Sulfur-containing amide type organic molybdenum compound as well as preparation method and application thereof
The sulfamide-containing organic molybdenum compound is generated by the reaction of thiocarboxylic acid and amine compounds in an organic solvent, which solves the problem of insufficient friction reduction effect of nitrogen-containing organic molybdenum additives in the prior art, and realizes a green and environmentally friendly and efficient lubricating additive. Significantly improves friction and wear performance.
Patent Information
- Application Number
- CN202410871469.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-01
AI Technical Summary
The existing nitrogen-containing organic molybdenum additives still have room for improvement in friction reduction effects, and their environmental friendliness and environmental protection need to be further improved to meet the needs of green and environmentally friendly lubricating additives.
The sulfamide-containing organic molybdenum compound is formed by reacting thiocarboxylic acid and amine compounds in an organic solvent, and further reacting with the molybdenum compound at a specific temperature to prepare a structure of R1-S-C(=O)-N-R2 -Sulphamide-containing organic molybdenum compound of Mo-O-R3 is used as a lubricating grease additive. The method includes reacting at 60 to 150°C for 1 to 10 hours to form a sulfamide-containing organic ligand, and then reacting with the molybdenum compound at 100 to 180°C for 6 to 20 hours to form a highly efficient lubricating additive.
The method is simple in process and environmentally friendly, and the product has significant friction-reduction and anti-wear properties. It is suitable for lubricating greases, improves tribological properties, and shows excellent friction-reduction effects under different loads and addition amounts.
Smart Images

Figure CN118909000A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lubricating additives and relates to a sulfuramide-containing organic molybdenum compound and a preparation method and application thereof. Background Art
[0002] Friction and wear are one of the main factors that lead to energy loss, reduced energy utilization, increased material loss or damage. During the operation of mechanical equipment, adding appropriate friction reducers to reduce friction and wear of friction pairs can improve energy utilization and equipment life.
[0003] Molybdenum compounds have a long history as friction modifiers. Molybdenum disulfide was the first molybdenum compound used, but it is insoluble in lubricating oil, which greatly limits its application. Subsequently, oil-soluble organic molybdenum represented by dialkyl dithiophosphate molybdenum (Mo DDP) was developed and mainly used in existing related fields of internal combustion. However, although the presence of phosphorus effectively reduces metal friction, it can poison the three-way catalyst of automobile exhaust treatment devices. Therefore, the development of environmentally friendly organic molybdenum friction reducers has become the main research direction.
[0004] Chinese patent CN1 01029265A uses p-hydroxyphenyl alkyl acid polyol ester, inorganic molybdenum compound, and fatty amine, aromatic amine, mixed amine, amide or a mixture of any two or more of them to react and obtain a sulfur-free and phosphorus-free organic molybdenum lubricating additive.
[0005] US Patent No. 6,645,921 B2 uses oil, diamine and molybdenum compound to react in the absence of volatile organic solvent to form a product with high molybdenum content, and the reaction product can be used to remove unreacted molybdenum compound without filtering.
[0006] In summary, the nitrogen-containing organic molybdenum additives disclosed so far respond to the need for green and environmentally friendly lubricant additives, but their friction reduction effect needs to be further improved. Therefore, the invention of a green and environmentally friendly, highly efficient friction reduction lubricant additive has a positive impact on the field of lubricant grease technology. Summary of the invention
[0007] In view of the defects in the prior art, the first aspect of the present invention is to provide a sulfuramide-containing organic molybdenum compound.
[0008] The objective of the present invention is achieved through the following technical solutions:
[0009] The present invention provides a sulfuramide-containing organic molybdenum compound having the following structure:
[0010]
[0011] Where R1 is a C2-C3 straight chain or branched alkyl group, R2 is a C8-C 26 Straight chain or branched chain alkyl.
[0012] The second aspect of the present invention is to provide a method for preparing a sulfuramide-containing organic molybdenum compound, comprising the following steps:
[0013] (1) reacting mercaptocarboxylic acid, an organic solvent, and an amine compound at 60 to 150° C. for 1 to 10 hours to obtain a sulfuramide-containing organic ligand;
[0014] (2) reacting the sulfuramide-containing organic ligand and the molybdenum compound at 100 to 180° C. for 6 to 20 hours to obtain a sulfuramide-containing organic molybdenum compound.
[0015] The preparation method involves the following chemical equation:
[0016]
[0017] As a preferred option:
[0018] In step (1):
[0019] The amine compound is selected from aliphatic amine, aromatic amine or a mixed amine thereof.
[0020] The solvent is selected from any one of ethanol, methanol, propanol, tetrahydrofuran, dioxane, ethylene glycol, glycerol, acetone, N,N-dimethylformamide, benzene, toluene, xylene, petroleum ether, kerosene, etc., preferably petroleum ether and toluene.
[0021] The reaction temperature is preferably 80° C. and the reaction time is 4 hours.
[0022] In step (2):
[0023] The molybdenum compound is selected from an organic or inorganic molybdenum source, and is preferably any one of molybdenum trioxide, molybdenum acetylacetonate, ammonium molybdate, sodium molybdate, and the like.
[0024] The molar ratio of the oil-soluble organic carboxylate to the molybdenum source compound is 1:0.25-1, preferably 1:1.
[0025] The reaction temperature is preferably 130° C. and the reaction time is 10 hours.
[0026] The third aspect of the present invention is to provide a sulfur amide-type organic molybdenum compound for use as a lubricating grease additive.
[0027] As a preferred embodiment, the amount of the sulfuramide-type organic molybdenum compound added to the lubricating grease is 1 to 10 wt.%, preferably 1 to 4 wt.%, based on the weight of the lubricating grease.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) The present invention uses mercaptocarboxylic acid and aliphatic amine, aromatic amine, and mixed amine to react, which has a simple process, is easy to operate, and is environmentally friendly.
[0030] (2) The product has good tribological properties and can significantly improve the anti-friction and anti-wear properties as a lubricating grease additive. The present invention is further described below in conjunction with the accompanying drawings and specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:
[0032] Figure 1 is a schematic diagram of infrared spectrum analysis of the friction reducer 4n-MoTMP prepared in Example 1;
[0033] Figure 2 The friction reducing properties of the friction reducer 4n-MoTMP prepared in Example 1 with different addition amounts in urea-based grease;
[0034] Figure 3 The anti-wear properties of the friction reducer 4n-MoTMP prepared in Example 1 with different addition amounts in urea-based grease;
[0035] Figure 4 The friction reducing properties of the friction reducer 4n-MoTMP prepared in Example 1 are different when loaded in urea-based grease;
[0036] Figure 5 The friction reducer 4nMoTMP prepared in Example 1 has different anti-wear properties when loaded in urea-based grease. DETAILED DESCRIPTION
[0037] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0038] Example 1
[0039] 2.12 g of mercaptopropionic acid and 50 ml of petroleum ether solution were added to a 100 ml three-necked flask, 5.35 g of oleylamine (the molar ratio of mercaptopropionic acid to oleylamine was 1:1) was added, the mixture was heated to reflux at 80°C with stirring for 4 h, 0.72 g of molybdenum trioxide (the molar ratio of mercaptopropionic acid to molybdenum trioxide was 4:1) was added, the mixture was heated to reflux at 130°C with stirring for 10 h, there was no solid powder in the reaction solution, the reaction was terminated, the petroleum ether solvent was removed by distillation under reduced pressure after cooling to room temperature, and 6.51 g of dark yellow paste liquid was obtained, which was a sulfuramide-type organic molybdenum compound, marked as 4n-MoTMP, with a yield of 84.04%.
[0040] The above reaction equation:
[0041]
[0042] Product Confirmation:
[0043] FT-IR spectrum of the product (see Figure 1 )as follows:
[0044] 3312cm-1, NH stretching vibration absorption peak; 2921cm -1 , CH stretching vibration absorption peak: 1652cm-1, C=O stretching vibration absorption peak: 1458cm -1 , CN stretching vibration absorption peak; 714cm -1 , Mo-SC stretching vibration absorption peak.
[0045] Table 1. ICP test results of molybdenum and sulfur content of the product of Example 1
[0046] element Mo S Measured value (%) 6.20 6.02 .
[0047] Replacement Example
[0048] The preparation method is the same as that of Example 1, except that the reaction temperature of the sulfuramide-containing organic ligand and the molybdenum compound is adjusted, and its effect on the yield of the product of Example 1 is tested.
[0049] Table 2. Effect of reaction temperature on product yield of Example 1
[0050] Serial number Reaction temperature (℃) Yield (%) Example 1-1 100 60.41 Example 1-2 110 68.56 Examples 1-3 120 79.13 Examples 1-4 140 82.97 Examples 1-3 150 82.56 .
[0051] As shown in Table 2: When the temperature is low, the activity of the reactants is poor, and water molecules are not easy to leave the system, resulting in a low yield of the target product. As the reaction temperature increases, the positive progress of the amidation reaction is promoted, and the conversion rate of the reactants increases. However, when the temperature is too high, the yield of the product in Example 1 does not change significantly, so the optimal temperature is 130°C.
[0052] Example 2
[0053] 1.06 g of mercaptopropionic acid and 40 ml of petroleum ether solution were added to a 100 ml three-necked flask, and 2.68 g of oleylamine (the molar ratio of mercaptopropionic acid to oleylamine was 1:1) was added, and the mixture was heated to reflux at 80° C. with stirring for 4 h. 0.72 g of molybdenum trioxide (the molar ratio of mercaptopropionic acid to molybdenum trioxide was 2:1) was continued to be added, and the mixture was heated to reflux at 130° C. with stirring for 10 h. There was no solid powder in the reaction solution, and the reaction was terminated. After cooling to room temperature, the petroleum ether solvent was removed by distillation under reduced pressure to obtain 3.65 g of a dark yellow paste liquid, which was a sulfuramide-type organic molybdenum compound, marked as 2n-MoTMP, with a yield of 85.68%.
[0054] The above reaction equation:
[0055]
[0056] Table 3. ICP test results of molybdenum and sulfur content of the product of Example 2
[0057] element Mo S Measured value (%) 11.25 5.56 .
[0058] Application Example: Application of Sulfamide-containing Organic Molybdenum Compounds as Friction Reducers
[0059] According to NB / SH / T 0189-2017 and GB / T 3142-2019 standards, the sulfuramide-type organic molybdenum compound prepared in Example 1 was added to the base grease (urea-based grease) in different contents (the added amounts were the mass percentages of urea-based grease: 1%, 2%, 3%, and 4%, respectively), and after stirring evenly, the average friction coefficient (ACOF) and wear spot diameter (WSD) were measured.
[0060] The test method is as follows: using the MS-10J four-ball testing machine of Xiamen Tianji Automation Co., Ltd., the steel ball used is a second-level GCr15 standard steel ball (AISI-52100), with a diameter of 12.7mm and a hardness of 59-61HRC. The load is 392N, the temperature is 75℃, the test time is 60min, and the speed is 1200rpm. The test results are shown in Table 4:
[0061] Table 4. Tribological properties of Example 1 at different addition amounts in urea-based grease
[0062] Concentration of Example 1 (%) Average friction coefficient Wear spot diameter (mm) 0.0 0.0980 0.673 1.0 0.0786 0.505 2.0 0.0621 0.425 3.0 0.0787 0.413 4.0 0.0620 0.428 .
[0063] The MS-10J four-ball tester of Xiamen Tianji Automation Co., Ltd. was used, and the steel balls used were second-grade GCr15 standard steel balls (AISI-52100). In the base grease (urea-based grease), 2% by mass of the sulfur-containing amide type organic molybdenum compound prepared in Example 1 was added. The test was carried out at different loads at a temperature of 75°C, a test time of 60 minutes, and a rotation speed of 1200 rpm. The test results are shown in Table 5:
[0064] Table 5. Tribological properties of Example 1 with 2% addition under different loads
[0065] Load(N) Average friction coefficient Wear spot diameter (mm) 196 0.0992 0.392 294 0.0805 0.386 392 0.0621 0.425 490 0.0816 0.568 .
[0066] The results show that the sulfuramide-type organic molybdenum compound synthesized in the embodiment of the present invention can effectively reduce the friction coefficient (COF) and the wear spot diameter (WSD). The technical solution of the present invention has the following advantages: the process is green and environmentally friendly, the separation is simple and efficient, the friction reduction and anti-wear performance are excellent, and it has broad application prospects.
[0067] The present invention has many specific application paths, and the above is only a preferred embodiment of the present invention. It should be pointed out that the above embodiments are only used to illustrate the present invention, and are not used to limit the protection scope of the present invention. For those of ordinary skill in the art, several improvements can be made without departing from the principle of the present invention, and these improvements should also be regarded as the protection scope of the present invention.
Claims
1. A sulfuramide-containing organic molybdenum compound, the structural formula of which is as follows: Wherein: R1 is a C2-C3 straight chain or branched chain alkyl, R2 is a C8-C 26 Straight chain or branched chain alkyl.
2. A method for preparing the sulfuramide-containing organic molybdenum compound according to claim 1, characterized in that: The following steps are involved: (1) reacting mercaptocarboxylic acid, an organic solvent, and an amine compound at 60 to 150° C. for 1 to 10 hours to obtain a sulfuramide-containing organic ligand; (2) reacting the sulfuramide-containing organic ligand and the molybdenum compound at 100 to 180° C. for 6 to 20 hours to obtain a sulfuramide-containing organic molybdenum compound.
3. A method for preparing the sulfuramide-containing organic molybdenum compound according to claim 1, characterized in that: In step (1): the amine compound is selected from aliphatic amines, aromatic amines or a mixed amine thereof.
4. A method for preparing the sulfuramide-containing organic molybdenum compound according to claim 1, characterized in that: In step (1), the solvent is selected from any one of ethanol, methanol, propanol, tetrahydrofuran, dioxane, ethylene glycol, glycerol, acetone, N,N-dimethylformamide, benzene, toluene, xylene, petroleum ether and kerosene.
5. A method for preparing the sulfuramide-containing organic molybdenum compound according to claim 1, characterized in that: In step (1): the reaction temperature is 80° C. and the reaction time is 4 hours.
6. A method for preparing the sulfuramide-containing organic molybdenum compound according to claim 1, characterized in that: In step (2): the molybdenum compound is selected from an organic or inorganic molybdenum source.
7. A method for preparing the sulfuramide-containing organic molybdenum compound according to claim 1, characterized in that: In step (2): the molybdenum compound is selected from any one of molybdenum trioxide, molybdenum acetylacetonate, ammonium molybdate and sodium molybdate.
8. A method for preparing the sulfuramide-containing organic molybdenum compound according to claim 1, characterized in that: In step (2): the molar ratio of the oil-soluble organic carboxylate to the molybdenum source compound is 1:0.25-1.
9. A method for preparing the sulfuramide-containing organic molybdenum compound according to claim 1, characterized in that: In step (2): the reaction temperature is 130° C. and the reaction time is 10 hours.
10. Use of the sulfuramide-type organic molybdenum compound according to claim 1 as a lubricating grease additive.
Citation Information
Patent Citations
High-sulfur phosphorus-free trinuclear molybdenum compound, its preparation method and application
CN102382142A
Preparation of a sulfurized molybdenum amide complex and additive compositions having low residual active sulfur
CN102510866A
Non-sulfur and non-phosphorus organic molybdenum compound and preparation method and application thereof
CN104844656A
Preparation method and application of oil-soluble organic molybdenum catalyst precursor
CN118218026A