Method for relieving scaling of emulsion polymerization reactor and anti-scaling coating material
By applying an anti-scaling coating composed of hydrophilic monomers and crosslinked monomers on the inner wall and the surface of the emulsion polymerization reactor, the problem of scaling of the emulsion polymerization reactor is solved, and the durability and adhesion of the reactor are improved. , maintains the heat dissipation ability and product quality.
Patent Information
- Application Number
- CN202411075541.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-08
AI Technical Summary
Emulsion polymerization reactors are prone to scale during polymerization, resulting in a decrease in heat dissipation capacity and product quality. The durability and adhesion of existing anti-scaling methods are insufficient, which easily leads to weakening of the effect after repeated batches.
Apply an anti-scaling coating composed of hydrophilic monomers and crosslinked monomers to the inner wall of the reactor and the surface of the attachment. The anti-scaling layer with a thickness of between 1 nanometer and 10 microns is formed by chemical vapor deposition technology to improve adhesion and durability.
It significantly reduces the scaling phenomenon of the emulsion polymerization reactor, maintains the heat dissipation capacity of the reactor, extends the product yield, and maintains the integrity of the coating under multiple reaction conditions, preventing the impact of the dirt on in-situ detection.
Smart Images

Figure CN118909161A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for alleviating scaling of an emulsion polymerization reactor and an anti-scaling coating material, belonging to the technical field of emulsion polymerization anti-scaling. Background Art
[0002] Polymerization reactions include bulk polymerization, solution polymerization, emulsion polymerization, and suspension polymerization. Among them, emulsion polymerization is the process of dispersing monomers in water with the help of emulsifiers and mechanical stirring to form an emulsion, and then adding an initiator to initiate the polymerization of the monomers. Emulsion polymerization has a fast polymerization rate and a high molecular weight; water is generally used as a dispersion medium, which is relatively low in cost; the viscosity of the reaction system is relatively low, which is conducive to heat transfer and temperature control and is easier to control. However, during the reaction, the polymer emulsion may agglomerate due to the loss of local stability, forming microscopic or macroscopic coagulant dirt. These coagulant dirt may be deposited on the inner wall of the reactor and accessories that are in direct contact with the monomers, such as the stirring device, internal heat exchanger, thermometer sleeve or other parts. The monomer adsorbed on the reactor may also undergo polymerization reaction and continue to thicken. This phenomenon is called sticking to the reactor or glue hanging.
[0003] Scaling of polymerization reactors will reduce the heat dissipation capacity of polymerization reactions; polymer scale separation from the surface will affect the quality of polymer products. Severe scaling requires shutdown for cleaning. For intermittent emulsion polymerization reactors, cleaning will extend the non-production time. For continuous reactors, shutdown is required. These operations affect the output of polymers. Therefore, the development of anti-scaling methods for polymerization reactors has important industrial value.
[0004] At present, the known methods for preventing polymer from scaling on the inner wall of the polymerization container include adding an organic solvent to the polyacetal preparation solution (CN106905499A), etc. However, this method requires adding an organic solvent before each reaction, which consumes a large amount of solvent. A more reported method is to coat the inner wall and accessories of the reactor with a scaling inhibitor. The first reported scaling inhibitor is a polar compound such as an amine compound (US3515709A), but the durability of this polar compound is poor, the coating is easily damaged, and the effect will weaken after repeated polymerization batches exceed 5-6 times.
[0005] Therefore, researchers improved polar compound inhibitors into polymer scale inhibitors, such as condensation products of aromatic amine compounds and aromatic nitro compounds, including naphthoquinone dye components (CN1059151A), condensation products of aromatic amines and aromatic tetracarboxylic anhydrides (CN1079476A), tannin and acyl halide product coatings (CN1047301A); condensation products prepared under alkaline conditions by the reaction of aldehyde compounds, hydroxy aromatic compounds and aromatic compounds with sulfonic acid groups or carboxylic acid ester groups (IN201714045000); scale inhibitors obtained by applying the condensation products of formaldehyde and naphthol compounds to the reactor surface, etc. These polymer scale inhibitors have a relatively good anti-scaling effect, and the number of applicable polymerization reaction repetitions is increased compared to polar compounds, but they also have their own disadvantages: antifouling agents containing naphthoquinone and aromatic amine compounds are colored, and if the antifouling agents are peeled off during use, there may be a risk of dyeing the polymer; polymer scale will occur at the interface between the gas phase and the liquid phase inside the polymerization container. In addition, most of the antifouling coatings currently developed cannot be grafted to the substrate surface and have poor adhesion to the substrate. The detached coating may enter the latex and affect the product quality. Summary of the invention
[0006] In order to solve the above problems, the present invention provides a method for alleviating scaling of an emulsion polymerization reactor and a corresponding anti-scaling coating material, which can effectively inhibit scaling during the emulsion polymerization reaction.
[0007] The specific technical solutions are as follows:
[0008] The first object of the present invention is to provide a method for alleviating reactor fouling during an emulsion polymerization reaction, by applying an anti-fouling coating on the inner wall of the reactor and the surface of the reactor accessories, wherein the anti-fouling coating is polymerized from any one or two of a hydrophilic monomer and a cross-linking monomer.
[0009] In one embodiment of the present invention, the hydrophilic monomer is selected from any one or more of the following: acrylic monomers, acrylate monomers, acrylamide monomers, vinyl pyrrolidone, and 4-vinyl pyridine.
[0010] In one embodiment of the present invention, the molecular structure of the acrylic acid ester monomer is as follows:
[0011] R1 and R2 are independently selected from hydrogen, C 1-8 Alkyl, C 1-8 Alkoxy, C 2-10 Alkenyl or C 2-10 At least one of the alkynyl groups.
[0012] In one embodiment of the present invention, the molecular structure of the acrylamide monomer is as follows:
[0013] R3, R4, and R5 are independently selected from hydrogen, C 1-8 Alkyl, C 1-8 Alkoxy, C 2-10 Alkenyl or C 2-10 At least one of the alkynyl groups.
[0014] In one embodiment of the present invention, the molecular structure of vinyl pyrrolidone is
[0015] In one embodiment of the present invention, the molecular structure of 4-vinylpyridine is
[0016] In one embodiment of the present invention, the crosslinking monomer includes a monomer containing two or more vinyl groups.
[0017] In one embodiment of the present invention, the crosslinking monomer includes, but is not limited to, one or more of ethylene glycol dimethacrylate, diethylene glycol divinyl ether, divinyl benzene, siloxane monomers containing two or more vinyl groups, and the like.
[0018] In one embodiment of the present invention, the anti-fouling coating is preferably formed by polymerizing a cross-linking monomer, or by polymerizing a hydrophilic monomer and a cross-linking monomer, and more preferably by polymerizing a hydrophilic monomer and a cross-linking monomer.
[0019] In one embodiment of the present invention, when the hydrophilic monomer and the cross-linking monomer are copolymerized, the ratio of the hydrophilic monomer to the cross-linking monomer is 0.1:100-100:0.1.
[0020] In one embodiment of the present invention, the thickness of the anti-fouling coating is between 1 nanometer and 10 micrometers.
[0021] In one embodiment of the present invention, the material of the reactor includes but is not limited to metal, ceramic, quartz, glass, polymer and any composite material thereof.
[0022] In one embodiment of the present invention, the emulsion polymerization reaction includes an acrylate / styrene emulsion system, a vinyl acetate emulsion system, and the like.
[0023] In one embodiment of the present invention, a method for alleviating reactor fouling during an emulsion polymerization reaction specifically comprises the following steps:
[0024] (1) Pretreatment: The substrate is exposed to plasma or UV / ozone for a period of time to generate hydroxyl groups on the surface; then it is exposed to a silane coupling agent or a methyl radical precursor;
[0025] (2) Polymer deposition: The substrate is then exposed to an environment containing a hydrophilic monomer and / or a cross-linking monomer and an initiator to deposit an anti-fouling coating.
[0026] The plasma in step (1) includes oxygen plasma, ozone plasma, argon plasma, etc.
[0027] The pretreatment method in step (1) is to graft reactive groups onto the surface of the substrate or to activate oxygen free radicals on the surface.
[0028] The general structural formula of the silane coupling agent is RSiX3, where R is a group reactive with a hydrophilic monomer or a crosslinking monomer (such as an amino group, an epoxy group, a vinyl group, a methyl propionyl group, etc.), and X is -Cl, or C 1-4 Alkoxy (such as methoxy, ethoxy, etc.) The silane coupling agent can be selected from any one or more of the following: trichlorovinylsilane, 3-(methacryloyloxy)propyltrimethoxysilane, vinyltriethoxysilane, vinyltri(2-methoxyethoxy)silane, etc.
[0029] The methyl radical precursor includes any one or more of the following: di-tert-butyl peroxide, di-tert-amyl peroxide, tert-butyl peroxide, hydrogen peroxide, isobutyl phosphine.
[0030] The gas phase surface activation method includes using methyl radicals to abstract hydrogen from hydroxyl groups to generate oxygen radical sites on the surface.
[0031] The free radicals that can initiate polymerization in step (2) include azo free radicals, peroxide free radicals, perfluoroalkyl free radicals, dimethylamino free radicals, alkyl free radicals, and the like.
[0032] The deposition method in step (2) is induced chemical vapor deposition (iCVD).
[0033] During the chemical vapor deposition process, the flow rate of the hydrophilic monomer and / or the cross-linking monomer is 0.1-100 sccm.
[0034] During the chemical vapor deposition process, the flow rate of the initiator is 0.1-10 sccm.
[0035] During the chemical vapor deposition process, the pressure is controlled at 20-1000 mTorr; the temperature of the heating wire is controlled at 200-300°C.
[0036] The second object of the present invention is to provide a polymer for alleviating scaling during emulsion polymerization, wherein the polymer is polymerized from any one or both of a hydrophilic monomer and a cross-linking monomer.
[0037] The hydrophilic monomer and the crosslinking monomer are defined as above, respectively.
[0038] In one embodiment of the present invention, the polymer is preferably formed by polymerizing a cross-linking monomer, or by polymerizing a hydrophilic monomer and a cross-linking monomer, and more preferably by polymerizing a hydrophilic monomer and a cross-linking monomer.
[0039] In one embodiment of the present invention, the hydrophilic monomer is selected from any one or more of 4-vinylpyridine, hydroxyethyl methacrylate, N,N-dimethylacrylamide, and glycidyl methacrylate; the cross-linking monomer is selected from any one or more of diethylene glycol divinyl ether, trimethyl trivinyl cyclosiloxane, and ethylene glycol dimethacrylate.
[0040] In one embodiment of the present invention, the polymer may specifically include: 4-vinylpyridine / diethylene glycol divinyl ether copolymer, 1,3,5-trivinyl-1,3,5-trimethylcyclotrisiloxane / hydroxyethyl methacrylate copolymer, N,N-dimethylacrylamide / ethylene glycol dimethacrylate copolymer, 1,3,5-trivinyl-1,3,5-trimethylcyclotrisiloxane / glycidyl methacrylate copolymer.
[0041] The third object of the present invention is to provide an anti-fouling reactor for alleviating fouling during emulsion polymerization, comprising a reactor substrate and an anti-fouling coating, wherein the anti-fouling coating means the above-mentioned polymer.
[0042] The present invention also provides an emulsion polymerization reaction method, wherein the reaction is carried out in the above-mentioned anti-fouling reactor. The method can prevent polymer fouling and deposition during the emulsion polymerization process.
[0043] Beneficial effects:
[0044] According to the present invention, after the inner wall and accessory surfaces of the emulsion polymerization reactor are coated with the polymer anti-fouling coating material prepared by the present invention, the scaling is significantly reduced compared to the uncoated reactor; and the coating can still remain intact under multiple harsh polymerization reaction conditions (reaction temperature of about 80°C). This shows that the polymer anti-fouling coating prepared by the method of the present invention has good durability and adhesion. In addition, after using the method of the present invention, the heat dissipation capacity of the reactor is maintained, and there is no need to clean the reactor after each polymerization reaction, which greatly improves the output of the product.
[0045] For the windows of online detection devices such as in-situ Raman, the iCVD method of depositing the coating does not affect the original light transmittance, and can achieve a good anti-scaling effect, thereby preventing dirt from affecting in-situ detection. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is a light microscope image of the original 316L stainless steel;
[0047] Figure 2 This is a light microscope image of scaling on the surface of 316L with p(4VP-co-DEGDVE) coating;
[0048] Figure 3 This is a light microscope image of scaling on the 316L surface without p(4VP-co-DEGDVE) coating;
[0049] Figure 4 The adhesion test results of p(V3D3-co-HEMA) coating;
[0050] Figure 5 The infrared spectrum results of p(V3D3-co-HEMA) coating before and after 10 anti-fouling tests;
[0051] Figure 6 Schematic diagram of scaling at the gas-liquid interface in Example 2;
[0052] Figure 7 The absorbance comparison of the quartz glass surface before and after the scaling experiment in Example 5.
[0053] Figure 8 It is a schematic diagram of the polymer antifouling coating of the present invention preventing scale from adhering to the wall surface of the emulsion polymerization reactor. DETAILED DESCRIPTION
[0054] Example 1
[0055] The anti-fouling coating of 4-vinylpyridine and diethylene glycol divinyl ether (p(4VP-co-DEGDVE)) polymer was prepared by iCVD vapor phase method and used in the actual butyl acrylate / styrene emulsion polymerization process to observe the effect.
[0056] The p(4VP-co-DEGDVE) copolymer coating was deposited by iCVD method. The specific preparation method is as follows:
[0057] The silicon wafer and 316 stainless steel substrate were exposed to oxygen plasma for 5-60 minutes, and then placed in an iCVD chamber. The substrate was exposed to di-tert-butyl peroxide (TBPO, 97%). When the heating wire temperature was higher than 270°C, TBPO would undergo heterolysis to produce methyl radicals, which could capture hydrogen atoms from surface hydroxyl groups and activate oxygen radicals on the surface.
[0058] The anti-fouling coating was then deposited in an iCVD reactor using commercially available 4-vinylpyridine (4VP) and diethylene glycol divinyl ether (DEGDVE) as monomers and di-tert-butyl peroxide as an initiator. During the deposition process, 4VP and DEGDVE monomers were heated to 40-90°C to generate sufficient vapor pressure for delivery to the chamber, and the flow rates of the two monomers were controlled at 0.1-100 sccm and 0.1-100 sccm, respectively. The initiator was kept at room temperature, and the flow rate of the initiator was controlled at 0.1-10 sccm. The chamber pressure was controlled at 20-1000 mTorr by a butterfly valve. The temperature of the heating wire was controlled at 200-300°C, and the sample stage was controlled at 20-80°C by a constant temperature water bath.
[0059] The adhesion between the coating and the substrate is tested using the 100-grid method. A sharp blade with a 1 mm interval is used to cut lines in the coating for testing (ASTM D3359). Then 3M Transparent Tape 600 is pasted in the 100-grid. The 3M tape is quickly pulled up. The adhesion of the coating can be tested by calculating the proportion of the coating area adhered by the tape to the total area. The edges of the cut can remain completely smooth after 30 tests, and there is no peeling on the edges of the grid. The ASTM grade can reach the highest 5B level. The increased adhesion improves the durability of the antifouling coating and prevents the paint from falling off and contaminating the emulsion.
[0060] Antifouling experiment: The obtained stainless steel with p(4VP-co-DEGDVE) coating and the uncoated stainless steel were placed in a 1L reactor at the same time, and the reactor was also filled with butyl acrylate / styrene emulsion as shown in Table 1. The temperature was maintained at 80°C with a water bath, and stirred at 200 rpm for 15 hours. The mass change of the stainless steel before and after the test was weighed with an electronic balance (Mettler Telodo, accuracy 0.01 mg). The mass change of the stainless steel substrate without the iCVD protective layer before and after the test was 12800.3 μg / cm 2 The mass change of the stainless steel substrate with p(4VP-co-DEGDVE) coating before and after the test was 998.4 μg / cm 2 , compared with the stainless steel without protective layer, the scaling is slowed down by 92.2%. Figure 1-3 As shown in the optical microscope image, the amount of dirt on the surface deposited with p(4VP-co-DEGDVE) coating is significantly reduced, showing good anti-fouling performance. And the stainless steel with p(4VP-co-DEGDVE) coating can effectively prevent scaling at the gas-liquid interface.
[0061] Table 1 Butyl acrylate / styrene emulsion polymerization formula
[0062]
[0063] The above antifouling experiment was repeated on stainless steel with p(4VP-co-DEGDVE) coating and stainless steel without coating, each time for 15 hours. After the reaction, the stainless steel sheet was taken out and dried with a nitrogen gun, and the experiment was repeated 10 times. The results showed that the structure of the coating was not destroyed and still maintained a good antifouling effect.
[0064] Example 2
[0065] The anti-fouling coating of 1,3,5-trivinyl-1,3,5-trimethylcyclotrisiloxane and hydroxyethyl methacrylate (p(V3D3-co-HEMA)) polymer was prepared by iCVD vapor phase method and used in the actual butyl acrylate / styrene emulsion polymerization process to observe the effect.
[0066] The p(V3D3-co-HEMA) copolymer coating was deposited by iCVD method. The specific preparation method is as follows:
[0067] The silicon wafer and 316L stainless steel were exposed to oxygen plasma for 5-60 min and then immersed in trichlorovinyl silane for 2-12 h to graft a layer of vinyl on the surface.
[0068] The p(V3D3-co-HEMA) film was deposited on silicon wafers and 316L stainless steel surfaces in an iCVD reactor. Purchased V3D3 and hydroxyethyl methacrylate were used as monomers, and di-tert-butyl peroxide (TBPO, 97%) was used as an initiator. During the deposition process, V3D3 and HEMA monomers were heated to 30-80°C to generate sufficient vapor pressure to be delivered to the chamber, and the flow rates of the two monomers were controlled at 0.1-100sccm and 0.1-100sccm, respectively. The initiator was kept at room temperature, and the flow rate of the initiator was controlled at 0.1-10sccm. The chamber pressure was controlled at 20-1000mTorr by a butterfly valve. The temperature of the heating wire was controlled at 200-300°C, and the sample stage was controlled at 20-80°C by a constant temperature water bath.
[0069] The adhesion between the coating and the substrate is tested using the 100-grid method. A sharp blade with a 1 mm interval is used to cut lines in the coating for testing (ASTM D3359). Then 3M Transparent Tape 600 is pasted on the 100-grid. The 3M tape is quickly pulled up. The adhesion of the coating can be tested by calculating the proportion of the coating area adhered by the tape to the total area. Figure 4 The optical microscope image shows that the edges of the cuts remain completely smooth after 30 tests, with no peeling on the edges of the lattice, and the ASTM grade can reach the highest 5B level. The increased adhesion improves the durability of the antifouling coating, preventing the paint from falling off and contaminating the emulsion.
[0070] The obtained stainless steel with p(V3D3-co-HEMA) coating and the uncoated stainless steel were placed in a 1L reactor at the same time, and the reactor was also filled with butyl acrylate / styrene emulsion as shown in Table 1. The temperature was maintained at 80°C with a water bath, and stirred at 200 rpm for 6 hours. The mass change of the stainless steel before and after the test was weighed with an electronic balance (Mettler Telodo, accuracy 0.01 mg). The mass change of 316 stainless steel without iCVD protective layer before and after the test was 2162.4 μg / cm 2 The mass change of 316 stainless steel with p(V3D3-co-HEMA) coating before and after the test is 432.8μg / cm 2 , compared with the stainless steel without protective layer, the scaling is slowed down by 80.0%.
[0071] The above antifouling experiment was repeated on stainless steel with p(V3D3-co-HEMA) coating and stainless steel without coating, each time for 6 hours. After the reaction, the stainless steel sheet was taken out and dried with a nitrogen gun. The experiment was repeated 10 times. The infrared spectra of the coating before and after the experiment are shown in Figure 2. Figure 5 As shown in the figure, the structure of the coating was not destroyed. In the 10th reaction, the mass change of 316 stainless steel without iCVD protective layer before and after the test was 3429.5 μg / cm 2 The mass change of 316 stainless steel with p(V3D3-co-HEMA) coating before and after the test is 451.6μg / cm 2 Compared with the stainless steel without protective layer, the scaling was slowed down by 86.8%, and the anti-fouling effect of the coating was still maintained after 10 reactions.
[0072] The coating can effectively prevent scaling at the gas-liquid interface, such as Figure 6 As shown. In the figure, 3# and 4# stainless steels are pictures of stainless steels deposited with p(V3D3-co-HEMA) coating after an anti-scaling test, and 1# and 2# are pictures of stainless steels without coating after an anti-scaling test. The red frame is the gas-liquid interface of the emulsion, indicating that the polymer antifouling coating can effectively prevent scaling at the interface.
[0073] Example 3
[0074] The anti-fouling coating of divinylbenzene and vinylpyrrolidone (p(DVB-co-NVP)) polymer was prepared by iCVD vapor phase method and its effect was observed in the actual vinyl acetate emulsion polymerization process.
[0075] The p(DVB-co-NVP) copolymer coating was deposited by iCVD method. The specific preparation method is as follows:
[0076] The silicon wafer and 304 stainless steel were exposed to oxygen plasma for 5-60 min and then immersed in trichlorovinyl silane for 2-12 h to graft a layer of vinyl on the surface.
[0077] The p(DVB-co-NVP) thin film was deposited on silicon wafers and 304 stainless steel surfaces in an iCVD reactor. Commercially available DVB and NVP were used as monomers, and di-tert-butyl peroxide (TBPO, 97%) was used as an initiator. During the deposition process, the DVB and NVP monomers were heated to 40-90°C to generate sufficient vapor pressure to be delivered to the chamber, and the flow rates of the two monomers were controlled at 0.1-100 sccm and 0.1-100 sccm, respectively.
[0078] The initiator is kept at room temperature, and the flow rate of the initiator is controlled at 0.1-10 sccm. The chamber pressure is controlled at 20-1000 mTorr by a butterfly valve. The temperature of the heating wire is controlled at 200-300°C, and the sample stage is controlled at 20-80°C by a constant temperature water bath.
[0079] The obtained stainless steel with p(DVB-co-NVP) coating and the uncoated stainless steel were placed in a 1L reactor at the same time, and the reactor was also filled with vinyl acetate emulsion as shown in Table 2. The temperature was maintained at 80°C with a water bath, and stirred at 200 rpm for 15 hours. The mass change of the stainless steel before and after the test was weighed with an electronic balance (Mettler Telodo, accuracy 0.01 mg). The mass change of 304 stainless steel without iCVD protective layer before and after the test was 5466.9 μg / cm 2 The mass change of 304 stainless steel with p(DVB-co-NVP) coating before and after the test is 967.4μg / cm 2 , compared with the stainless steel without protective layer, the scaling is slowed down by 82.3%.
[0080] Table 2 Vinyl acetate emulsion polymerization formula
[0081]
[0082] Example 4
[0083] The anti-fouling coating of N,N-dimethylacrylamide and ethylene glycol dimethacrylate (p(DMAAm-co-EGDMA)) polymer was prepared by iCVD vapor phase method and its effect was observed in the actual butyl acrylate / styrene emulsion polymerization process.
[0084] The p(DMAAm-co-EGDMA) copolymer coating was deposited by iCVD method. The specific preparation method is as follows:
[0085] The silicon wafer and 304 stainless steel were exposed to oxygen plasma for 5-60 minutes, and then placed in an iCVD chamber. The substrate was exposed to di-tert-butyl peroxide (TBPO, 97%). When the heating wire temperature was higher than 270°C, TBPO would undergo heterolysis to produce methyl radicals, which could capture hydrogen atoms from surface hydroxyl groups and activate oxygen radicals on the surface.
[0086] Subsequently, p(DMAAm-co-EGDMA) thin films were deposited on silicon wafers and 304 stainless steel surfaces in an iCVD reactor. Purchased N,N-dimethylacrylamide (DMAAm) and ethylene glycol dimethacrylate (EGDMA) were used as monomers, and di-tert-butyl peroxide was used as an initiator. During the deposition process, DMAAm and EGDMA monomers were heated to 40-90°C to generate sufficient vapor pressure to be delivered to the chamber, and the flow rates of the two monomers were controlled at 0.1-100 sccm and 0.1-100 sccm, respectively. The initiator was kept at room temperature, and the flow rate of the initiator was controlled at 0.1-10 sccm. The chamber pressure was controlled at 20-1000 mTorr by a butterfly valve. The temperature of the heating wire was controlled at 200-300°C, and the sample stage was controlled at 20-80°C by a constant temperature water bath.
[0087] The obtained stainless steel with p(DMAAm-co-EGDMA) coating and the uncoated stainless steel were placed in a 1L reactor at the same time, and the reactor was also filled with polybutyl acrylate / styrene emulsion as shown in Table 1. The temperature was maintained at 80°C with a water bath, and stirred at 200 rpm for 12 hours. The mass change of the stainless steel before and after the test was weighed with an electronic balance (Mettler Telodo, accuracy 0.01 mg). The mass change of 304 stainless steel without iCVD protective layer before and after the test was 7789.3 μg / cm 2 The mass change of 304 stainless steel with p(DMAAm-co-EGDMA) coating before and after the test is 1098.3μg / cm 2 , compared with the stainless steel without protective layer, the scaling is slowed down by 85.9%.
[0088] Example 5
[0089] The anti-fouling coating of glycidyl methacrylate and V3D3 (p(GMA-co-V3D3)) polymer was prepared by iCVD vapor phase method and used in the actual butyl acrylate / styrene emulsion polymerization process to observe the effect.
[0090] The p(GMA-co-V3D3) copolymer coating was deposited by iCVD method. The specific preparation method is as follows:
[0091] The silicon wafer and quartz substrate are exposed to UV / ozone for 5-60 minutes, and then placed in an iCVD chamber. The substrate is exposed to di-tert-butyl peroxide (TBPO, 97%). When the heating wire temperature is higher than 270°C, TBPO will undergo heterolysis to produce methyl radicals, which can capture hydrogen atoms from surface hydroxyl groups and activate oxygen radicals on the surface.
[0092] The p(GMA-co-V3D3) film was then deposited on silicon wafers and quartz surfaces in an iCVD reactor. Purchased glycidyl methacrylate (GMA) and V3D3 were used as monomers, and di-tert-butyl peroxide was used as an initiator. During the deposition process, GMA and V3D3 monomers were heated to 40-90°C to generate sufficient vapor pressure to be delivered to the chamber, and the flow rates of the two monomers were controlled at 0.1-100sccm and 0.1-100sccm, respectively. The initiator was kept at room temperature, and the flow rate of the initiator was controlled at 0.1-10sccm. The chamber pressure was controlled at 20-1000mTorr by a butterfly valve. The temperature of the heating wire was controlled at 200-300°C, and the sample stage was controlled at 20-80°C by a constant temperature water bath.
[0093] The obtained quartz with p(GMA-co-V3D3) coating and uncoated quartz were placed in a 1L reactor at the same time, and the reactor was also filled with butyl acrylate / styrene emulsion as shown in Table 1. The temperature was maintained at 80°C with a water bath, and stirred at 200 rpm for 8 hours. The mass change of the quartz substrate before and after the experiment was weighed with an electronic balance (Mettler Telodo, accuracy 0.01 mg). The mass change of the quartz substrate without iCVD protective layer before and after the experiment was 3459.9 μg / cm 2 The mass change of the quartz substrate with p(GMA-co-V3D3) coating deposited on the surface before and after the test is 928.4μg / cm 2 , compared with the quartz scaling without protective layer, it is slowed down by 73.2%.
[0094] The absorbance of the deposited and undeposited anti-fouling coating quartz was measured using a UV-visible spectrophotometer. Figure 7 As shown. After deducting the original substrate background, the absorbance of the undeposited anti-scaling coating is 0.125, and the absorbance of the deposited anti-scaling coating is 0.01, and the absorbance change is reduced by more than 12 times. The transmittance of the quartz without the anti-scaling coating decreased by 25.0%, while the transmittance of the quartz with the anti-scaling coating only decreased by 2.3%.
[0095] Example 6
[0096] Siloxane polymer antifouling coating was prepared by initiated chemical vapor deposition (iCVD) and its effect was observed in the actual butyl acrylate / styrene emulsion polymerization process.
[0097] The polytrimethyltrivinylcyclosiloxane (pV3D3) coating was deposited by iCVD method. The specific preparation method is as follows:
[0098] The silicon wafer and 316L stainless steel were exposed to oxygen plasma for 5-60 min and then immersed in trichlorovinyl silane for 12 h to graft a layer of vinyl on the surface.
[0099] The silicon wafer and 316L stainless steel were then transferred to the iCVD reactor, using purchased 1,3,5-trivinyl-1,3,5-trimethylcyclotrisiloxane (V3D3,>95%) as a monomer and di-tert-butyl peroxide (TBPO, 97%) as an initiator. During the deposition process, the V3D3 monomer was heated to 50-80°C to generate sufficient vapor pressure to be delivered to the chamber, the initiator was kept at room temperature, and the flow rates of the monomer and initiator were controlled at 0.1-10sccm and 0.1-10sccm, respectively. The chamber pressure was controlled at 20-1000mTorr by a butterfly valve. The temperature of the heating wire was controlled at 200-300°C, and the sample stage was controlled at 20-80°C by a constant temperature water bath.
[0100] The obtained 316 stainless steel with pV3D3 coating and the 316 stainless steel without iCVD protective layer were placed in a 1L reactor at the same time. The reactor was also filled with butyl acrylate / styrene emulsion as shown in Table 1. The temperature was maintained at 80°C with a water bath, stirred at 200 rpm for 4 hours, and the mass change of the stainless steel before and after the test was weighed with an electronic balance (Mettler Telodo, accuracy 0.01 mg). The mass change of the 316 stainless steel without iCVD protective layer before and after the test was 131 μg / cm 2 The mass change of pV3D3 coating deposited on 316 stainless steel surface is 37μg / cm 2 , compared with the stainless steel without protective layer, the scaling is slowed down by 71.8%.
[0101] The embodiments provided above are not intended to limit the scope of the present invention, and the steps described are not intended to limit the execution order thereof. Those skilled in the art may make obvious improvements to the present invention in combination with existing common knowledge, which also fall within the scope of protection defined by the claims of the present invention.
Claims
1. A method for alleviating reactor fouling during an emulsion polymerization reaction, wherein an anti-fouling coating is applied to the inner wall of the reactor and the surface of the reactor accessories, wherein the anti-fouling coating is polymerized from any one or both of a hydrophilic monomer and a cross-linking monomer.
2. The method according to claim 1, characterized in that The hydrophilic monomer is selected from any one or more of the following: acrylic monomers, acrylate monomers, acrylamide monomers, vinyl pyrrolidone, and 4-vinyl pyridine.
3. The method according to claim 1, characterized in that The crosslinking monomers include monomers containing two or more vinyl groups.
4. The method according to claim 1, characterized in that: The cross-linking monomer is selected from any one or more of the following: ethylene glycol dimethacrylate, diethylene glycol divinyl ether, divinyl benzene, and a siloxane monomer containing two or more vinyl groups.
5. The method according to claim 1, characterized in that The anti-fouling coating is formed by polymerizing a cross-linking monomer, or by polymerizing a hydrophilic monomer and a cross-linking monomer.
6. The method according to claim 1, characterized in that The thickness of the anti-fouling coating is between 1 nanometer and 10 micrometers.
7. The method according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: (1) Pretreatment: The substrate is exposed to plasma or UV / ozone for a period of time to generate hydroxyl groups on the surface; then it is exposed to a silane coupling agent or a methyl radical precursor; (2) Polymer deposition: The substrate is then exposed to an environment containing a hydrophilic monomer and / or a cross-linking monomer and an initiator to deposit an anti-fouling coating.
8. The method according to claim 7, characterized in that The plasma includes oxygen plasma, ozone plasma, and argon plasma; the general structural formula of the silane coupling agent is RSiX3, where R is a group reactive with a hydrophilic monomer or a crosslinking monomer, and X is -Cl or C 1-4 Alkoxy; the methyl radical precursor includes one or more of the following: di-tert-butyl peroxide, di-tert-amyl peroxide, tert-butyl peroxide, hydrogen peroxide, isobutyl phosphine.
9. A polymer for alleviating scaling during emulsion polymerization, characterized in that: The polymer is copolymerized by a hydrophilic monomer and a crosslinking monomer; wherein the hydrophilic monomer is selected from any one or more of 4-vinylpyridine, hydroxyethyl methacrylate, N,N-dimethylacrylamide, and glycidyl methacrylate; and the crosslinking monomer is selected from any one or more of diethylene glycol divinyl ether, trimethyltrivinylcyclosiloxane, and ethylene glycol dimethacrylate.
10. An anti-fouling reactor for alleviating fouling during emulsion polymerization, characterized in that: The invention comprises a reactor substrate and an anti-fouling coating, wherein the anti-fouling coating comprises the polymer according to claim 9.
Citation Information
Patent Citations
Method for coating a substrate using plasma
CN101048237A
Metal coating of objects using plasma polymerisation
CN103328686A
Method of preventing polymer scale deposition during polymerization
CN1045399A
Polymer scale preventive agent, polymerization vessel for preventing polymer scale deposition, and process of producing using said vessel
CN1061977A
Resistance-reducing and antifouling coating composition and resistance-reducing and antifouling coating prepared from same
CN107400438A
Cited By
Polyurea-based super-infiltration anti-scaling coating and preparation method thereof
CN120098517A