Ionic polymer resin with high saponification degree as well as preparation method and application thereof

By controlling the molar ratio of ethylene-unsaturated carboxylic acid ester copolymer and alkali, the problem of large amounts of salt impurities and three waste emissions under high saponification rate in the saponification method is solved, and an ionic polymer resin with high saponification degree and excellent physical properties is achieved.

CN118909164APending Publication Date: 2024-11-08JIANGSU SAILBOAT PETROCHEMICAL CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410971095.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the preparation of ionic polymer resins by saponification, high saponification rate requirements lead to the use of a large number of alkalis and acids, resulting in a large number of salt impurities and three wastes, which increases the difficulty of cleaning and the water absorption of the material, and reduces transparency.

Method used

By controlling the molar ratio of ethylene-unsaturated carboxylic acid ester copolymer and alkali in the range of 1:(1.05-1.1), the amount of alkali is used, the generation of metal salt impurities and the emission of three wastes are reduced, while ensuring high saponification and excellent Physical and chemical properties.

Benefits of technology

The ionic polymer resin with high saponification degree is achieved, which reduces water absorption and waste emissions, improves transparency, and ensures high saponification degree and excellent physical and chemical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004953235510000081
    Figure BDA0004953235510000081
  • Figure BDA0004953235510000091
    Figure BDA0004953235510000091
Patent Text Reader

Abstract

The invention provides ionic polymer resin with high saponification degree and a preparation method and application thereof, the ionic polymer resin is obtained by reacting ethylene-unsaturated carboxylic ester copolymer and alkali in a mixed solvent, and the molar ratio of the ethylene-unsaturated carboxylic ester copolymer to the alkali is 1: (1.05-1.1); the molar ratio of the ethylene-unsaturated carboxylic ester copolymer to the alkali is controlled to be within the specific range, so that the relative dosage of the alkali is greatly reduced, the generation of metal salt impurities is reduced, the emission of three wastes is further reduced, and the production cost is reduced. And the obtained ionic polymer resin can be ensured to have relatively high saponification degree and excellent physical and chemical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ionic polymers, and in particular relates to an ionic polymer resin with a high saponification degree and a preparation method and application thereof. Background Art

[0002] Due to its excellent transparency, wear and scratch resistance, low-temperature impact toughness and chemical resistance, ionomer resins are widely used in sports equipment such as golf, bowling, sleds, surfboards, cosmetics and perfume containers, food packaging (especially vacuum skin packaging), glass lamination (high-rise, photovoltaic glass for construction), automotive parts, polar exploration equipment and other fields.

[0003] At present, saponification is one of the main preparation methods of ionomer resins, which has the advantages of easy availability of base resin and good product uniformity compared with neutralization method. The ionomer resin prepared by saponification is prepared by using ethylene-unsaturated carboxylic acid ester copolymer as base resin, and is prepared in the form of solution through steps such as alkaline saponification, acid demetallization, purification and desalting. For example, CN113993909A discloses an ionomer resin, which comprises: (meth) acrylic acid unit (A), (meth) acrylic acid neutralizer unit (B), and ethylene unit (C), and all monomer units constituting the aforementioned ionomer resin are used as a reference, and the total content of the aforementioned unit (A) and the aforementioned unit (B) is 6 to 10 mol%, and the content of the salt formed by the strong acid and the strong base in the aforementioned ionomer resin is 1 to 400 mg / kg.

[0004] However, the saponification step of the ionomer resin produced by the saponification process generally requires that the saponification rate of the resin reach more than 99%, so a large amount of alkali is added, which in turn leads to the need to add a large amount of acid in the demetallization step and produce a large amount of salt. The production of a large amount of salt impurities will increase the difficulty of cleaning and produce a large amount of three wastes. On the other hand, the residual salt will increase the water absorption of the ionomer resin and reduce its transparency.

[0005] Therefore, in view of the above technical problems, it is urgent to develop an ionic polymer resin with a high saponification degree and which can effectively reduce the discharge of three wastes. Summary of the invention

[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide an ionic polymer resin with a high saponification degree and a preparation method and application thereof, by controlling the molar ratio of the ethylene-unsaturated carboxylic acid ester copolymer and the alkali to be 1: (1.05-1.1), thereby greatly reducing the relative amount of alkali, reducing the generation of metal salt impurities, and thereby reducing the discharge of three wastes, while also ensuring that the obtained ionic polymer resin has a high saponification degree and excellent physical and chemical properties.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides an ionomer resin with a high saponification degree, wherein the ionomer resin is obtained by reacting an ethylene-unsaturated carboxylic acid ester copolymer and a base in a mixed solvent;

[0009] The molar ratio of the ethylene-unsaturated carboxylic acid ester copolymer to the base is 1:(1.05-1.1), for example, 1:1.06, 1:1.07, 1:1.08, 1:1.09 or 1:1.1.

[0010] The ionic polymer resin with high saponification degree provided by the present invention is obtained by reacting ethylene-unsaturated carboxylic acid ester copolymer and alkali in a mixed solvent, and the molar ratio of the ethylene-unsaturated carboxylic acid ester copolymer to the alkali is 1:(1.05-1.1); the present invention controls the molar ratio of the ethylene-unsaturated carboxylic acid ester copolymer to the alkali within the above-mentioned specific range, on the one hand, greatly reducing the relative amount of alkali, reducing the generation of metal salt impurities, thereby reducing the discharge of three wastes, reducing the water absorption of the obtained ionic polymer resin, and improving its transparency; on the other hand, it can ensure that the obtained ionic polymer resin has a high saponification degree; if the molar ratio of the ethylene-unsaturated carboxylic acid ester copolymer to the alkali is too small, it is easy to cause the obtained ionic polymer resin to have a low saponification degree, and if the molar ratio of the ethylene-unsaturated carboxylic acid ester copolymer to the alkali is too large, it is easy to cause excessive generation of metal salt impurities, thereby increasing the discharge of three wastes.

[0011] In the present invention, the “ionic polymer resin with a high saponification degree” refers to an ionic polymer resin with a saponification degree of ≥ 99%.

[0012] Preferably, based on the total mass of the ethylene-unsaturated carboxylate copolymer, the base and the mixed solvent as 100%, the mass of the ethylene-unsaturated carboxylate copolymer is 10-50%, for example 10%, 20%, 30%, 40% or 50%.

[0013] Preferably, the mass percentage of the unsaturated carboxylate structural unit in the ethylene-unsaturated carboxylate copolymer is 7 to 35%;

[0014] Preferably, the melt index of the ethylene-unsaturated carboxylate copolymer is 5 to 300 g / 10 min, for example, 5 g / 100 min, 10 g / 100 min, 50 g / 100 min, 100 g / 100 min, 150 g / 100 min, 200 g / 100 min, 250 g / 100 min or 300 g / 100 min, and more preferably 20 to 150 g / 10 min; the test temperature of the above melt index is 190° C. and the load is 2.16 kg.

[0015] Preferably, the ethylene-unsaturated carboxylic acid ester copolymer includes ethylene-butyl acrylate copolymer and / or ethylene-methyl methacrylate copolymer, and more preferably ethylene-butyl acrylate copolymer (EnBA). The advantage of selecting EnBA as the resin matrix is ​​that the raw materials are available and the price is relatively low.

[0016] Preferably, the alkali comprises sodium hydroxide and / or potassium hydroxide, more preferably sodium hydroxide.

[0017] Preferably, the mixed solvent comprises a combination of an alcohol solvent and an aromatic solvent.

[0018] Preferably, the mass ratio of the alcohol solvent to the aromatic solvent is (1-7):(9-3), such as 1:9, 2:8 or 3:7.

[0019] Preferably, the alcohol solvent includes any one of methanol, ethanol, tert-butanol, n-butanol or isopropanol, or a combination of at least two thereof, and methanol is more preferably used.

[0020] Preferably, the aromatic solvent includes any one of p-xylene, o-xylene, m-xylene, xylene, and toluene, or a combination of at least two of them, and more preferably xylene and / or p-xylene.

[0021] Preferably, the reaction temperature is ≥160°C, for example 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C or 200°C, etc., more preferably ≥170°C, and even more preferably ≥180°C. If the reaction temperature is too low, it is easy to result in a low degree of saponification of the obtained ionic polymer resin.

[0022] Preferably, the saponification degree of the unsaturated carboxylic acid ester in the ionomer resin is ≥99%, such as 99%, 99.1%, 99.2%, 99.3%, 99.4%, 99.5%, 99.6%, 99.7%, 99.8% or 99.9%, etc.; the saponification degree is obtained by FTIR-ATR characterization, and the scanning range is 400-4000cm -1 , resolution 4cm -1 , scanning times 32 times; the formula is saponification degree = 1-A1 / A2 / (S1 / S2), where A1 is the ionomer resin at 1735cm in the infrared spectrum. -1 The peak area at (corresponding to the C=O double bond stretching vibration peak in the ester group) is 3000-2800 cm -1 The peak area at 1735 cm-1 in the infrared spectrum of the ethylene-unsaturated carboxylic acid ester copolymer corresponding to the ionic polymer resin is shown in Figure 2 (corresponding to the CH stretching vibration peak).-1 The peak area at (corresponding to the C=O double bond stretching vibration peak in the ester group), S2 is 3000~2800cm -1 The peak area at (corresponding to the CH stretching vibration peak).

[0023] In a second aspect, the present invention provides a method for preparing an ionic polymer resin with a high saponification degree as described in the first aspect. The preparation method comprises: reacting an ethylene-unsaturated carboxylic acid ester copolymer, a base and a mixed solvent, and drying to obtain the ionic polymer resin with a high saponification degree.

[0024] Preferably, the reaction temperature is ≥160°C, for example 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C or 200°C, etc., more preferably ≥170°C, and even more preferably ≥180°C.

[0025] Preferably, the reaction time is 0.5 to 6 h, for example 0.5 h, 1 h, 2 h, 3 h, 4 h, 5 h or 6 h.

[0026] Preferably, the reaction pressure is 0-10 MPa, such as 0 MPa, 2 MPa, 4 MPa, 6 MPa, 8 MPa or 10 MPa.

[0027] Preferably, after the reaction is completed, the step of adding methanol for precipitation is further included.

[0028] In a third aspect, the present invention provides a use of the ionic polymer resin with a high saponification degree as described in the first aspect in the preparation of sports equipment, cosmetic containers, food packaging materials, glass laminates, automotive parts or polar exploration equipment.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The ionic polymer resin with high saponification degree provided by the present invention is obtained by reacting an ethylene-unsaturated carboxylic acid ester copolymer and an alkali in a mixed solvent, and the molar ratio of the ethylene-unsaturated carboxylic acid ester copolymer to the alkali is 1:(1.05-1.1); the present invention controls the molar ratio of the ethylene-unsaturated carboxylic acid ester copolymer to the alkali within the above-mentioned specific range, thereby not only greatly reducing the relative amount of alkali, reducing the generation of metal salt impurities, and reducing the discharge of three wastes, but also ensuring that the saponification degree of the obtained ionic polymer resin reaches more than 99.0% and the content of metal salt impurities is less than 1%. DETAILED DESCRIPTION

[0031] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only used to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0032] Some of the raw material information involved in the following examples and comparative examples are as follows:

[0033] (1) Ethylene-butyl acrylate copolymer (EnBA)

[0034] EnBA20020: melt index is 20 g / 10 min, 190°C, the mass percentage of butyl acrylate structural unit is 20%, purchased from Repsol, brand name E20020;

[0035] EnBA27150: melt index is 150 g / 10 min, 190°C, the mass percentage of butyl acrylate structural unit is 27%, purchased from Repsol, brand E27150;

[0036] EnBA33150: melt index is 150 g / 10 min, 190° C., the mass percentage of butyl acrylate structural unit is 33%, purchased from Repsol, brand number E33150.

[0037] (2) Anhydrous methanol: AR grade, Sinopharm Reagent.

[0038] (3) p-Xylene: AR grade, Sinopharm Reagent.

[0039] (3) Sodium hydroxide: NaOH, AR grade, Sinopharm Reagent.

[0040] Example 1

[0041] A high-saponification ionic polymer resin, the preparation method of which comprises: placing 30g of ethylene-butyl acrylate copolymer EnBA27150, 24g of p-xylene, 6g of methanol and 2.65g of sodium hydroxide in a reactor, stirring and heating to 180°C, reacting at 2MPa for 4h and then terminating the reaction, adding excess methanol for precipitation, filtering and vacuum drying to obtain the ionic polymer resin.

[0042] Example 2

[0043] A high-saponification ionic polymer resin, the preparation method of which comprises: placing 15g of ethylene-butyl acrylate copolymer EnBA27150, 48g of p-xylene, 12g of methanol and 1.33g of sodium hydroxide in a reactor, stirring and heating to 180°C, reacting at 2MPa for 4h and then terminating the reaction, adding excess methanol for precipitation, filtering and vacuum drying to obtain the ionic polymer resin.

[0044] Example 3

[0045] A high-saponification ionic polymer resin, the preparation method of which comprises: placing 25.8g of ethylene-butyl acrylate copolymer EnBA27150, 54g of p-xylene, 6g of methanol and 2.39g of sodium hydroxide in a reactor, stirring and heating to 180°C, reacting at 2MPa for 4h and then terminating the reaction, adding excess methanol for precipitation, filtering and vacuum drying to obtain the ionic polymer resin.

[0046] Example 4

[0047] A high saponification degree ionic polymer resin, which differs from Example 3 in that the amount of p-xylene used is 18 g, the amount of methanol used is 42 g, and other substances, amounts and parameters are the same as those in Example 3.

[0048] Example 5

[0049] A high saponification degree ionomer resin, which differs from Example 3 in that 48 g of xylene is used to replace 54 g of p-xylene, and the amount of methanol used is 12 g, and other substances, amounts and parameters are the same as those in Example 3.

[0050] Example 6

[0051] A high-saponification ionic polymer resin, the preparation method of which comprises: placing 25.8g of ethylene-butyl acrylate copolymer EnBA33150, 48g of p-xylene, 12g of methanol and 2.92g of sodium hydroxide in a reactor, stirring and heating to 180°C, reacting at 2MPa for 4h and then terminating the reaction, adding excess methanol for precipitation, filtering and vacuum drying to obtain the ionic polymer resin.

[0052] Example 7

[0053] A high-saponification ionic polymer resin, the preparation method of which comprises: placing 25.8g of ethylene-butyl acrylate copolymer EnBA20020, 48g of p-xylene, 12g of methanol and 1.69g of sodium hydroxide in a reactor, stirring and heating to 180°C, reacting at 1MPa for 4h and then terminating the reaction, adding excess methanol for precipitation, filtering and vacuum drying to obtain the ionic polymer resin.

[0054] Example 8

[0055] An ionic polymer resin with a high saponification degree, which differs from Example 7 only in that the reaction time is 2 hours, and other substances, amounts and parameters are the same as those in Example 7.

[0056] Example 9

[0057] An ionic polymer resin with a high saponification degree, which differs from Example 7 only in that the reaction time is 1 hour, and other substances, amounts and parameters are the same as those in Example 7.

[0058] Example 10

[0059] An ionic polymer resin with a high saponification degree, which differs from Example 1 in that the reaction temperature is 170° C., and other substances, amounts and parameters are the same as those in Example 1.

[0060] Embodiment 11

[0061] An ionic polymer resin with a high saponification degree, which differs from Example 1 in that the reaction temperature is 160° C., and other substances, amounts and parameters are the same as those in Example 1.

[0062] Example 12

[0063] An ionic polymer resin with a high saponification degree, which differs from Example 1 in that the reaction temperature is 150° C., and other substances, amounts and parameters are the same as those in Example 1.

[0064] Comparative Example 1

[0065] An ionomer resin, which differs from Example 1 in that the amount of sodium hydroxide used is 2.5 g, and other substances, amounts and parameters are the same as those in Example 1.

[0066] Comparative Example 2

[0067] An ionomer resin, which differs from Example 1 in that the amount of sodium hydroxide used is 3.04 g, and other substances, amounts and parameters are the same as those in Example 1.

[0068] Performance Test:

[0069] (1) Saponification degree: characterized by FTIR-ATR, scanning range 400~4000cm -1 , resolution 4cm -1 , scanning times 32 times; the formula is saponification degree = 1-A1 / A2 / (S1 / S2); where A1 is 1735cm in the infrared spectrum of the ionic polymer resin -1 The peak area at (corresponding to the C=O double bond stretching vibration peak in the ester group) is 3000-2800 cm -1 The peak area at 1735 cm-1 (corresponding to the CH stretching vibration peak) is shown in Figure 2. S1 is the peak area at 1735 cm-1 in the infrared spectrum of the precursor EnBA resin corresponding to the ionomer resin. -1 The peak area at (corresponding to the C=O double bond stretching vibration peak in the ester group), S2 is 3000~2800cm -1 The peak area at (corresponding to the CH stretching vibration peak).

[0070] (2) Metal residue: The metal residue in the ionomer resin was tested using an ion chromatograph (CIC-D160), specifically the anion content of the metal compound, such as chloride ion, sulfate ion, etc.

[0071] The ionomer resins provided in Examples 1 to 12 and Comparative Examples 1 to 2 were tested according to the above test method. The test results are shown in Table 1:

[0072] Table 1

[0073]

[0074]

[0075] From the data in Table 1, we can see that:

[0076] The saponification degree of the ionic polymer resins provided in Examples 1 to 9 is higher than 99.0%, and the metal salt impurity content is 0.31-1%, which not only greatly reduces the relative amount of alkali, but also reduces the production of metal salt impurities; while the saponification degree of the ionic polymer resin provided in Comparative Example 1 is only 98%, and the metal salt impurity content in the ionic polymer resin provided in Comparative Example 2 is as high as 1.7%, both of which do not meet the requirements;

[0077] Comparing the data of Example 1 with those of Examples 10 to 12, it can be seen that the reaction temperature also affects the saponification degree of the obtained ionomer resin. Too low a reaction temperature will lead to a decrease in the saponification degree.

[0078] The applicant declares that the present invention illustrates a high saponification degree ionomer resin and its preparation method and application through the above embodiments, but the present invention is not limited to the above embodiments, that is, it does not mean that the present invention must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. An ionomer resin with a high saponification degree, characterized in that: The ionomer resin is obtained by reacting an ethylene-unsaturated carboxylic acid ester copolymer and a base in a mixed solvent; The molar ratio of the ethylene-unsaturated carboxylic acid ester copolymer to the base is 1:(1.05-1.1).

2. The ionomer resin according to claim 1, characterized in that Based on the total mass of the ethylene-unsaturated carboxylate copolymer, the base and the mixed solvent as 100%, the mass of the ethylene-unsaturated carboxylate copolymer is 10 to 50%; Preferably, the mass percentage of the unsaturated carboxylate structural unit in the ethylene-unsaturated carboxylate copolymer is 7 to 35%; Preferably, the melt index of the ethylene-unsaturated carboxylic acid ester copolymer is 5 to 300 g / 10 min, more preferably 20 to 150 g / 10 min; Preferably, the ethylene-unsaturated carboxylic acid ester copolymer includes ethylene-butyl acrylate copolymer and / or ethylene-methyl methacrylate copolymer, and more preferably ethylene-butyl acrylate copolymer.

3. The ionomer resin according to claim 1 or 2, characterized in that: The base includes sodium hydroxide and / or potassium hydroxide, preferably sodium hydroxide.

4. The ionomer resin according to any one of claims 1 to 3, characterized in that The mixed solvent includes a combination of an alcohol solvent and an aromatic solvent; Preferably, the mass ratio of the alcohol solvent to the aromatic solvent is (1-7):(9-3); Preferably, the alcohol solvent includes any one of methanol, ethanol, tert-butanol, n-butanol or isopropanol, or a combination of at least two thereof, and methanol is more preferably used; Preferably, the aromatic solvent includes any one of p-xylene, o-xylene, m-xylene, xylene, and toluene, or a combination of at least two of them, and more preferably xylene and / or p-xylene.

5. The ionomer resin according to any one of claims 1 to 4, characterized in that The reaction temperature is ≥160°C, preferably ≥170°C, more preferably ≥180°C.

6. The ionomer resin according to any one of claims 1 to 5, characterized in that The saponification degree of the ionomer resin is ≥99%.

7. A method for preparing an ionomer resin with a high saponification degree as claimed in any one of claims 1 to 6, characterized in that: The preparation method comprises: reacting ethylene-unsaturated carboxylic acid ester copolymer, alkali and mixed solvent, and drying to obtain the ionic polymer resin with high saponification degree.

8. The preparation method according to claim 7, characterized in that: The reaction temperature is ≥160°C, preferably ≥170°C, and more preferably ≥180°C; Preferably, the reaction time is 0.5 to 6 hours; Preferably, the reaction pressure is 0-10 MPa.

9. The preparation method according to claim 7 or 8, characterized in that: The method further comprises adding methanol for precipitation after the reaction.

10. Use of the ionomer resin with a high saponification degree as claimed in any one of claims 1 to 6 in the preparation of sports equipment, cosmetic containers, food packaging materials, glass laminates, automobile parts or polar exploration equipment.