High-temperature-resistant thickening agent for fracturing fluid and preparation method of high-temperature-resistant thickening agent

By copolymerizing the polymerizable amphiphilic monomer after reacting N,N,N',N'-tetramethylbenzidine and bromopropylene in the fracturing liquid, acrylamide and dimethylaminoethyl methacrylate, an amphiphilicity is formed by copolymerizing the polymerizable amphiphilic monomer with acrylamide and dimethylaminoethyl methacrylate in the fracturing liquid. The thickener of the structure solves the problems of insufficient high temperature resistance and shear resistance in the prior art, achieves viscosity adaptability and reduced surface activity, and improves the production capacity of oil and gas wells.

CN118909183APending Publication Date: 2024-11-08SICHUAN YINYU CHEM TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410950544.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing fracturing fluid has insufficient high temperature and shear resistance, and its viscosity does not have environmental adaptability, which affects the stable production and increase production of oil and gas wells.

Method used

The polymerizable amphiphilic monomer is prepared by reacting N,N,N',N'-tetramethylbenzidine with bromopropylene, and copolymerized with acrylamide and dimethylaminoethyl methacrylate to form a non-polar phenyl group. amphiphilic structure thickeners of polar quaternary ammonium groups have adaptive viscosity adjustment and surfactivity.

Benefits of technology

It improves the viscosity adaptability, high temperature and shear resistance of the fracturing fluid, reduces the pipeline fluid resistance, increases the construction displacement and transformation volume, and increases the production capacity of oil and gas wells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909183A_ABST
    Figure CN118909183A_ABST
Patent Text Reader

Abstract

The invention discloses a high-temperature-resistant thickening agent for fracturing fluid and a preparation method of the high-temperature-resistant thickening agent. The high-temperature-resistant thickening agent has a structure as shown in a formula A, the preparation method of the high-temperature-resistant thickening agent for the fracturing fluid comprises the following steps: (1) reacting N, N, N ', N'-tetramethyl benzidine with bromopropene to prepare a polymerizable amphiphilic monomer; and (2) carrying out copolymerization on acrylamide, the polymerizable amphiphilic monomer and dimethylaminoethyl methacrylate to prepare the high-temperature-resistant thickening agent for the fracturing fluid. The viscosity of the high-temperature-resistant thickening agent for the fracturing fluid can change along with the environment, and the high-temperature-resistant thickening agent is high in adaptability, high-temperature-resistant and high in shear resistance. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of oilfield chemistry and engineering technology, and in particular to a high temperature resistant thickener for fracturing fluid and a preparation method thereof. Background Art

[0002] In the process of oil extraction, fracturing is an important technical means to stabilize and increase the production of oil and gas wells. The cracks created by fracturing can improve the conductivity, change the seepage state of the fluid, reduce energy loss, and thus increase the production of oil wells. Fracturing refers to the injection of a suitable fluid into the developed reservoir by applying high pressure through ground equipment. When the pressure exceeds the formation fracture pressure, the fluid will split the reservoir to create cracks, while carrying proppants and spreading into the cracks. After the pressure is released and the fluid breaks the gel and returns to the formation, the proppants fill the newly created cracks to form a fluid channel with high conductivity, thereby improving the production capacity of oil and gas wells or enhancing the injection capacity of water wells.

[0003] In the prior art, hydraulic fracturing is mainly used for fracturing, and fracturing fluid is used as the working fluid in the process of hydraulic fracturing to transform oil and gas reservoirs. Its performance directly affects the success or failure of fracturing construction and the effect of increasing the production of reservoirs after fracturing. At present, fracturing fluids include natural plant gums, plant gums, cellulose and other natural polymer materials. Among them, natural plant gums have a lot of residues after gel breaking, which blocks the proppant filling layer and causes artificial cracks, and their use is limited; natural polymer materials such as plant gums and cellulose have disadvantages such as poor high-temperature stability and cannot be fractured in high-temperature environments. In order to improve the performance of fracturing fluids, synthetic water-soluble fracturing fluids have become a hot research direction at home and abroad. The commonly used polymers in synthetic water-soluble fracturing fluids are mainly polyacrylamide, methylene polyacrylamide, etc. Compared with natural plant gums, they have the advantages of strong thickening ability, insensitivity to bacteria, good gel stability, strong sand suspension ability, no residue, and no damage to the formation. However, the performance of synthetic polymers in the prior art is relatively fixed, the adaptability is insufficient, and the high temperature resistance and shear resistance are not well met.

[0004] Therefore, there is an urgent need for a high-temperature resistant thickener for fracturing fluid that has a viscosity that can change with the environment, has strong adaptability, and is resistant to high temperatures and shear. Summary of the invention

[0005] Purpose of the invention: In view of the defects of the prior art, the purpose of the present invention is to provide a high temperature resistant thickener for fracturing fluid, which has a viscosity that can change with the environment, has strong adaptability, and is resistant to high temperature and shear, and a preparation method thereof.

[0006] Technical solution:

[0007] A high temperature resistant thickener for fracturing fluid, the high temperature resistant thickener for fracturing fluid having a structure as shown in the following formula A:

[0008]

[0009] Among them, x:y:n=(40-50):(8-15):(5-10), and the molecular weight is 9 million to 12 million.

[0010] The high temperature resistant thickener for fracturing fluid provided by the present invention has a viscosity that can change with the environment, has strong adaptability, and has high temperature resistance and shear resistance.

[0011] The method for preparing the high temperature resistant thickener for fracturing fluid comprises the following steps:

[0012] (1) N,N,N',N'-tetramethylbenzidine reacts with allyl bromide to prepare a polymerizable amphiphilic monomer;

[0013] (2) acrylamide, a polymerizable amphiphilic monomer and dimethylaminoethyl methacrylate are copolymerized to prepare the high temperature resistant thickener for the fracturing fluid.

[0014] Furthermore, the specific method of step (1) is as follows: in a reactor, N,N,N',N'-tetramethylbenzidine and a solvent are added, stirred and mixed evenly, and under nitrogen protection, the temperature is raised to 35-45° C., and allyl bromide is slowly added dropwise for 2-3 hours. After the addition is completed, the temperature is raised to 50-55° C., and the reaction is kept warm for 18-24 hours, and the solvent is removed. After recrystallization, the polymerizable amphiphilic monomer is obtained.

[0015] The reaction process is:

[0016]

[0017] In the structure of the high temperature resistant thickener for fracturing fluid provided by the present invention, an amphiphilic structural monomer containing a non-polar benzene group and a polar quaternary ammonium group is polymerized. Based on its hydrophilic and lipophilic abilities, the obtained fracturing fluid thickener can reduce its own viscosity as the shearing effect increases, and can return to normal when the shearing effect disappears. It has the ability to adapt to the environment and has better tolerance.

[0018] Furthermore, the solvent is an alcohol solvent.

[0019] Furthermore, the molar ratio of the N,N,N',N'-tetramethylbenzidine to allyl bromide is 1:2.2-2.4.

[0020] In the high temperature resistant thickener structure for fracturing fluid provided by the present invention, the polymerized amphiphilic structure monomer has a certain surface activity, which can reduce the surface tension of the fracturing fluid and correspondingly reduce the fluid resistance of the pipeline, thereby increasing the construction displacement and the transformation volume.

[0021] Furthermore, the specific method of step (2) is as follows: in a reactor, acrylamide, polymerizable amphiphilic monomer and dimethylaminoethyl methacrylate are added in proportion and dissolved in water, nitrogen is introduced for 20-30 minutes, an initiator is added, the reactor is sealed, and adiabatic reaction is carried out, after the reaction is complete, the reaction is cooled to room temperature, and the product is washed, granulated and dried to obtain the high temperature resistant thickener for fracturing fluid.

[0022] The reaction process is:

[0023]

[0024] The high temperature resistant thickener for fracturing fluid provided by the present invention contains a large amount of amine groups, phenyl groups and multi-branched structures, and has a stable structure, so that the obtained fracturing fluid thickener can have stronger high temperature resistance and shear resistance.

[0025] Furthermore, the initiator is selected from one of azobisisobutyramidine hydrochloride and 2,2'-azabis(2-imidazoline) dihydrochloride.

[0026] Furthermore, the reaction temperature is 45-55° C. and the reaction time is 4-6 hours.

[0027] Furthermore, the total mass concentration of the acrylamide, the polymerizable amphiphilic monomer and dimethylaminoethyl methacrylate is 15%-25%.

[0028] When the total mass concentration of monomers is too low, there are fewer free radical monomers in the system, the reaction rate is slow, and the effective conversion rate of the system is low; when the total mass concentration of monomers is too high, the viscosity of the system will rise sharply in the self-acceleration stage of the polymerization reaction. At this time, the heat dissipation difficulty causes the local temperature of the system to be too high, and the amide groups in the polymer undergo intermolecular or intramolecular imidization cross-linking reactions, resulting in insoluble products.

[0029] Furthermore, the molar ratio of acrylamide, polymerizable amphiphilic monomer and dimethylaminoethyl methacrylate is (45-60):(5-10):(8-15).

[0030] Beneficial effects:

[0031] (1) In the structure of the high temperature resistant thickener for fracturing fluid provided by the present invention, an amphiphilic monomer containing a non-polar benzene group and a polar quaternary ammonium group is polymerized. Based on its hydrophilic and lipophilic abilities, the obtained fracturing fluid thickener can reduce its own viscosity as the shear effect increases, and can return to normal when the shear effect disappears. It has the ability to adapt to the environment and has better tolerance.

[0032] (2) In the high temperature resistant thickener structure for fracturing fluid provided by the present invention, the polymerized amphiphilic structure monomer has a certain surface activity, which can reduce the surface tension of the fracturing fluid and correspondingly reduce the fluid resistance of the pipeline, thereby increasing the construction displacement and improving the transformation volume.

[0033] (3) The structure of the high temperature resistant thickener for fracturing fluid provided by the present invention contains a large amount of amine groups, phenyl groups and multi-branched structures, and the structure is stable, so that the obtained high temperature resistant thickener for fracturing fluid has stronger high temperature resistance and shear resistance.

[0034] (4) The viscosity of the high temperature resistant thickener for fracturing fluid provided by the present invention can change with the environment, has strong adaptability, and has strong high temperature resistance and shear resistance. DETAILED DESCRIPTION

[0035] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0036] The commercially available fracturing fluid thickener is an oilfield chemical - oilfield fracturing thickener purchased from Suzhou Shunhua Changli Environmental Protection New Materials Co., Ltd.; the remaining reagents and equipment are conventional reagents and equipment in the technical field.

[0037] Example 1

[0038] Prepare the high temperature resistant thickener for fracturing fluid according to the following steps:

[0039] (1) In a four-necked flask equipped with a stirrer, a thermometer, a reflux condenser and a nitrogen protection device, 0.1 mol of N,N,N',N'-tetramethylbenzidine and 100 g of anhydrous ethanol are added, the mixture is uniformly mixed under stirring, nitrogen protection is introduced, the temperature is raised to 35° C., 0.22 mol of allyl bromide is slowly added dropwise for 2 hours, the temperature is raised to 50° C. after the addition is completed, the reaction is kept at this temperature for 18 hours, the anhydrous ethanol solvent is removed by rotary evaporation, a small amount of unreacted allyl bromide is washed away by water, the mixture is allowed to stand in a separatory funnel, the oil layer is separated, and the water layer is obtained. The water is removed by vacuum distillation, and the mixture is recrystallized with ethyl acetate / ethanol. The polymerizable amphiphilic monomer is separated and purified;

[0040] (2) In a flask equipped with a nitrogen protection device, 0.45 mol of acrylamide, 0.05 mol of a polymerizable amphiphilic monomer and 0.08 mol of dimethylaminoethyl methacrylate were added and dissolved in 300 ml of water, and nitrogen was introduced for 30 minutes. 4 g of azobisisobutylamidine hydrochloride was added, and the reactor was sealed, and the temperature was raised to 45° C. and the reaction was carried out by adiabatic insulation for 4 hours. After the reaction was completed, the reaction was cooled to room temperature, and the product was washed, granulated and dried to obtain the high temperature resistant thickener for fracturing fluid.

[0041] In its structure, x:y:n=42:8:5, and the molecular weight is 9 million.

[0042] Example 2

[0043] The method is basically the same as Example 1, except that in step (2), the molar amounts of acrylamide, polymerizable amphiphilic monomer and dimethylaminoethyl methacrylate are 0.5 mol, 0.1 mol and 0.15 mol respectively; and azobisisobutyramidine hydrochloride is replaced by 2,2'-azabis(2-imidazoline) dihydrochloride.

[0044] In its structure, x:y:n=45:15:10, and the molecular weight is 10 million.

[0045] Example 3

[0046] The method is basically the same as Example 1, except that in step (2), the molar ratios of acrylamide, polymerizable amphiphilic monomer and dimethylaminoethyl methacrylate are 0.6 mol, 0.08 mol and 0.1 mol respectively.

[0047] In its structure, x:y:n=50:10:8, and the molecular weight is 12 million.

[0048] Comparative Example 1

[0049] Commercially available fracturing fluid thickener.

[0050] Comparative Example 2

[0051] The process is basically the same as Example 1, except that the polymerizable amphiphilic monomer in step (2) is replaced by an equimolar amount of dimethylaminoethyl methacrylate.

[0052] Comparative Example 3

[0053] The process is basically the same as Example 1, except that in step (2), dimethylaminoethyl methacrylate is replaced by an equimolar amount of acrylamide.

[0054] Comparative Example 4

[0055] The process is basically the same as Example 1, except that in step (2), the molar ratios of acrylamide, polymerizable amphiphilic monomer and dimethylaminoethyl methacrylate are 0.3 mol, 0.1 mol and 0.2 mol respectively.

[0056] In its structure, x:y:n=25:20:10, and the molecular weight is 9 million.

[0057] Performance Testing

[0058] Weigh 965.5g of distilled water in a beaker and add the following substances in order: 5.5g of anhydrous calcium chloride, 4.5g of magnesium chloride, 20g of potassium chloride, and 58.5g of sodium chloride. After each reagent is completely dissolved, add another reagent to obtain mineralized water. The prepared reagents should be used immediately.

[0059] 1. Determination of apparent viscosity:

[0060] A beaker containing 400 mL of mineralized water was placed on a stirrer, the speed was adjusted to 400 r / min, 4.0 g of the samples of Examples 1-3 and Comparative Examples 1-4 were weighed and added to the mineralized water and stirred for 1 min to obtain a test solution, and a Fann-35 six-speed rotational viscometer was used to test the apparent viscosity of the test solution at a speed of 100 r / min.

[0061] 2. Shear resistance test:

[0062] A beaker containing 400 mL of mineralized water was placed on a stirrer, and the speed was adjusted to 400 r / min. 4.0 g of the samples of Examples 1-3 and Comparative Examples 1-4 were weighed and added into the mineralized water and stirred for 1 min to obtain a test solution. The test solution was placed on a variable frequency high-speed stirrer and stirred at 10000 r / min for 30 min. After the high-speed stirring was completed, a Fann-35 six-speed rotational viscometer was used to test the apparent viscosity of the test solution at a speed of 100 r / min.

[0063] 3. Recovery performance test after shearing:

[0064] After the shear resistance test, the solution to be tested was placed for 5 minutes, and then the apparent viscosity of the solution to be tested was measured at a rotation speed of 100 r / min using a Fann-35 six-speed rotational viscometer.

[0065] 4. High temperature resistance test:

[0066] A beaker containing 400 mL of mineralized water was placed on a stirrer, and the speed was adjusted to 400 r / min. 4.0 g of the samples of Examples 1-3 and Comparative Examples 1-4 were weighed and added to the mineralized water and stirred for 1 min to obtain a test solution. The test solution was placed in a 95° C. constant temperature heater. After 15 days, a Fann-35 six-speed rotational viscometer was used to test the apparent viscosity of the test solution at a speed of 100 r / min.

[0067] 5. Drag reduction rate detection:

[0068] A beaker containing 400 mL of mineralized water was placed on a stirrer, and the speed was adjusted to 400 r / min. 4.0 g of the samples of Examples 1-3 and Comparative Examples 1-4 were weighed and added into the mineralized water and stirred for 1 min to obtain the solution to be tested. Under the conditions of a pipe diameter of 10 mm and a temperature of 25°C, a JHIF-2 drag reduction instrument was used to detect the differential pressure of clean water and the above solutions as the displacement varied, and the maximum drag reduction rate as the displacement varied was calculated.

[0069] The test results are shown in the following table:

[0070]

[0071]

[0072] According to the comparison of the test results of Examples 1-3 and Comparative Example 1 in the above table, it can be seen that the high temperature resistant thickener for fracturing fluid provided by the present invention has stronger thickening ability, shear resistance and high temperature resistance than the commercially available fracturing fluid thickener; the viscosity of the high temperature resistant thickener for fracturing fluid provided by the present invention can be restored to the original viscosity after shearing, the viscosity loss is low, it has adaptability to environmental conditions, and has better tolerance; and the high temperature resistant thickener for fracturing fluid provided by the present invention has a certain drag reduction ability, which can reduce the surface tension of the fracturing fluid, correspondingly reduce the fluid resistance of the pipeline, thereby increasing the construction displacement and improving the transformation volume.

[0073] According to the comparison of the test results of Examples 1-3 and Comparative Example 2 in the above table, it can be seen that the amphiphilic structural monomer polymerized in the high temperature resistant thickener for fracturing fluid provided by the present invention, based on its simultaneous hydrophilic and lipophilic capabilities, can make the thickener have adaptive ability to the environment and better tolerance; and because the high temperature resistant thickener for fracturing fluid provided by the present invention has a certain surface activity, it can reduce the surface tension of the fracturing fluid and correspondingly reduce the fluid resistance of the pipeline.

[0074] According to the comparison of the test results of Examples 1-3 and Comparative Example 3 in the above table, it can be seen that the large amount of amine groups and multi-branched structures contained in the structure of the high-temperature resistant thickener for fracturing fluid provided by the present invention can make the high-temperature resistant thickener for fracturing fluid have stronger high-temperature resistance and shear resistance.

[0075] According to the comparison of the test results of Examples 1-3 and Comparative Example 4 in the above table, it can be seen that the polymerization degree between the monomers in the high temperature resistant thickener for fracturing fluid provided by the present invention has excellent performance within the ratio range provided by the present invention, and too low or too high will affect its performance.

[0076] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A high temperature resistant thickener for fracturing fluid, characterized in that: The high temperature resistant thickener for fracturing fluid has a structure as shown in the following formula A: Among them, x:y:n=(40-50):(8-15):(5-10), and the molecular weight is 9 million to 12 million.

2. The method for preparing the high temperature resistant thickener for fracturing fluid according to claim 1, characterized in that: The following steps are involved: (1) N,N,N',N'-tetramethylbenzidine reacts with allyl bromide to prepare a polymerizable amphiphilic monomer; (2) acrylamide, a polymerizable amphiphilic monomer and dimethylaminoethyl methacrylate are copolymerized to prepare the high temperature resistant thickener for the fracturing fluid.

3. The method for preparing a high temperature resistant thickener for fracturing fluid according to claim 2, characterized in that: The specific method of step (1) is as follows: in a reactor, N,N,N',N'-tetramethylbenzidine and a solvent are added, stirred and mixed evenly, heated to 35-45° C. under nitrogen protection, and allyl bromide is slowly added dropwise for 2-3 hours. After the addition is completed, the temperature is raised to 50-55° C., and the reaction is kept warm for 18-24 hours, and then the solvent is removed and the polymerizable amphiphilic monomer is obtained after recrystallization.

4. The method for preparing a high temperature resistant thickener for fracturing fluid according to claim 3, characterized in that: The solvent is an alcohol solvent.

5. The method for preparing a high temperature resistant thickener for fracturing fluid according to claim 3, characterized in that: The molar ratio of the N,N,N',N'-tetramethylbenzidine to allyl bromide is 1:2.2-2.

4.

6. The method for preparing a high temperature resistant thickener for fracturing fluid according to claim 2, characterized in that: The specific method of step (2) is as follows: in a reactor, acrylamide, polymerizable amphiphilic monomer and dimethylaminoethyl methacrylate are added in proportion and dissolved in water, nitrogen is introduced for 20-30 minutes, an initiator is added, the reactor is sealed, and adiabatic reaction is carried out, after the reaction is complete, the reactor is cooled to room temperature, and the product is washed, granulated and dried to obtain the high temperature resistant thickener for fracturing fluid.

7. The method for preparing a high temperature resistant thickener for fracturing fluid according to claim 6, characterized in that: The initiator is selected from one of azobisisobutyramidine hydrochloride and 2,2'-azabis(2-imidazoline) dihydrochloride.

8. The method for preparing a high temperature resistant thickener for fracturing fluid according to claim 6, characterized in that: The reaction temperature is 45-55°C; the reaction time is 4-6 hours.

9. The method for preparing a high temperature resistant thickener for fracturing fluid according to claim 6, characterized in that: The total mass concentration of the acrylamide, the polymerizable amphiphilic monomer and dimethylaminoethyl methacrylate is 15%-25%.

10. The method for preparing a high temperature resistant thickener for fracturing fluid according to claim 6, characterized in that: The molar ratio of acrylamide, polymerizable amphiphilic monomer and dimethylaminoethyl methacrylate is (45-60): (5-10): (8-15).