Self-healing high-adhesion eutectic solvent gel as well as preparation method and application thereof
By adding starch, nanochitin and polyvinyl alcohol to the eutectic solvent, a double-layer network was built, and the problems of hydrogel's vulnerability in harsh environments and high cost and high toxicity in ionic liquid gels were solved, and the The preparation of self-healing high adhesion eutectic solvent gel has good biocompatibility and mechanical properties.
Patent Information
- Application Number
- CN202410910816.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The performance of existing hydrogels is easily damaged in harsh environments, the synthesis of ionic liquid gels is high and toxic, and the molecular chain stretching of the polymer network is difficult to expand in low temperature environments, affecting the stability of the mechanical properties of the gel.
The eutectic solvent is prepared by hydrogen bond acceptor and hydrogen bond donor, polymerized monomer, crosslinking agent and initiator are added, and starch, nanochitin, and polyvinyl alcohol are added to the eutectic solvent, through a double-layer network Constructed to improve the adhesion and tensile strength of the gel to form a self-healing high adhesion and low eutectic solvent gel.
It has achieved the preparation of safe, non-toxic, excellent biocompatible, self-healing, adhesion, frost resistance and stable gel materials, which are suitable for biosensors, medical dressings, drug delivery vehicles and tissue engineering scaffolds.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of organic polymer compounds, and in particular to a self-healing high-adhesion eutectic solvent gel and a preparation method and application thereof. Background Art
[0002] Hydrogels and ionic liquid gels have attracted more and more attention in biosensors, medical dressings, drug delivery carriers, tissue engineering scaffolds, soil protection, etc. due to their advantages such as stretchability, high conductivity, and high transparency. Hydrogels are usually difficult to use in harsh environments, and both low and high temperatures will destroy the original properties of hydrogels. In contrast, ionic gels containing ionic liquids can withstand harsh environments, but synthetic ionic liquids are expensive and generally toxic, and there is a problem of ionic liquids leaking from ionic gels.
[0003] As a green solvent, deep eutectic solvents have the advantages of low cost, easy access, eco-friendliness, good biocompatibility, biodegradability, etc. They also have high design freedom, wide temperature resistance, good ionic conductivity, and strong solubility for many water-soluble or fat-soluble compounds. Therefore, the use of deep eutectic solvents to prepare polymer gels is one of the directions to solve the above-mentioned defects of ionic liquid gels.
[0004] For example, the Chinese invention patent with publication number CN117304396A discloses a self-hygroscopic low eutectic polymer gel and its application, wherein a hydrogen bond acceptor and a hydrogen bond donor are mixed in a certain proportion and heated to a transparent and clear liquid to prepare a low eutectic solvent, and then a monomer, a cross-linking agent and an ultraviolet light initiator are added to the low eutectic solvent, heated and stirred until uniformly dissolved, and a self-hygroscopic low eutectic polymer gel is obtained after curing under ultraviolet light. The low eutectic solvent provided by the invention is used as an ionic liquid in an ionic gel, so that the prepared self-hygroscopic low eutectic polymer gel not only has good thermal stability and mechanical properties, but also has good atmospheric hygroscopicity, and can absorb water vapor in the air for automatic hydration in a natural environment, and can desorb water at high temperature to achieve a water adsorption and desorption cycle.
[0005] Another example is the Chinese invention patent with publication number CN110054721A, which provides an application of a low eutectic solvent in ion gel, ion gel and preparation method, wherein the low eutectic solvent includes a hydrogen bond acceptor and a hydrogen bond donor with a molar ratio of 1:1.5-5.5, and the hydrogen bond donors are acrylic acid and maleic acid, which are used to improve the technical problem that the current low eutectic solvent is limited in the application of ion gel. The low eutectic solvent provided by the invention is used as an ionic liquid of ion gel, so that the prepared ion gel not only has good tensile properties and toughness, but also has high transparency, conductivity and self-healing function, and good environmental stability.
[0006] The preparation of the above ion gels relies on the support of the polymer matrix, and the development of its mechanical properties depends on the polymer network formed by cross-linking of monomers, which has a large room for improvement. In a freezing environment at a lower temperature, some areas of the molecular chain of the polymer network have difficulty in stretching or shrinkage, which will have an adverse effect on the gel morphology, stability and uniformity of mechanical properties. Therefore, providing a gel material with excellent mechanical properties, self-healing, adhesion, antifreeze and stability, safety and non-toxicity, and excellent biocompatibility is of great significance for expanding its application. Summary of the invention
[0007] In view of the above-mentioned defects of the prior art, in a first aspect of the present invention, a method for preparing a self-healing high-adhesion eutectic solvent gel with a simple process and green environmental protection is provided, comprising the following steps: (1) A low eutectic solvent formed by a hydrogen bond acceptor and a hydrogen bond donor is used as a gel dispersion medium, and a polymerization monomer, a crosslinking agent and an initiator are added thereto to obtain a precursor; (2) adding a suspension of a polyhydroxy reinforcing agent to the precursor, mixing, curing, and drying to obtain a self-healing high-adhesion eutectic solvent gel; Wherein, the polyhydroxy enhancer is selected from at least one of starch, nano-chitin and polyvinyl alcohol.
[0008] Preferably, in step (1), the hydrogen bond acceptor is choline chloride; and the hydrogen bond donor is selected from one or two of glycerol, ethylene glycol, urea, and citric acid.
[0009] Further preferably, the molar ratio of the hydrogen bond acceptor to the hydrogen bond donor is 1:1-2.
[0010] Further preferably, the preparation method of the deep eutectic solvent is as follows: mixing a hydrogen bond acceptor and a hydrogen bond donor at 80-95° C. to obtain a clear solution, and cooling to 30-50° C. to obtain a deep eutectic solvent.
[0011] Preferably, in step (1), the polymerizable monomer is acrylamide or acrylic acid.
[0012] Preferably, in step (1), the amount of the added polymerizable monomer accounts for 25%-30% of the mass of the low eutectic solvent.
[0013] Crosslinking agents and initiators are common additives used in polymer preparation. A crosslinking agent is a substance that can bridge linear molecules, thereby bonding multiple linear molecules to each other and crosslinking into a network structure. An initiator is a compound that can decompose under the action of light or heat to produce free radicals, which can further initiate polymerization reactions. Those skilled in the art can select a suitable type according to actual conditions. As presented in one or more embodiments of the present invention, N,N'-methylenebisacrylamide and ammonium persulfate can be selected as crosslinking agents and initiators.
[0014] Preferably, in step (1), the amount of the cross-linking agent added is 0.5‰-2‰ of the mass of the low eutectic solvent; and the amount of the thermal initiator added is 0.6‰-0.8‰ of the mass of the low eutectic solvent.
[0015] Preferably, in step (2), the amount of the polyhydroxy enhancer added is 10%-20% of the mass of the deep eutectic solvent.
[0016] In the present invention, the source of starch is not particularly limited, and ordinary starch or tapioca starch are all suitable types. Those skilled in the art can make a selection according to actual conditions. Gelatinization can be carried out in a conventional manner in the art, for example, an appropriate amount of acetic acid can be added as needed to promote gelatinization.
[0017] Preferably, in step (2), when starch is used as the polyhydroxy enhancer, the starch is pre-gelatinized at 70-90°C and then cooled to 40-50°C, and then the starch suspension is added to the precursor.
[0018] In actual preparation, the mixed solution is poured into the target mold, and after curing and drying, the gel material of the desired shape can be obtained. Based on the size and shape of the mold, technicians in this field can appropriately control the time at the curing temperature until the curing is completed. For small-scale preparation scenarios, a shorter curing time can be reasonably selected, such as stirring for 0.5-1 h under laboratory conditions; in the case of industrial-scale production, it can be appropriately extended to allow the gel to fully cure internally.
[0019] Preferably, in step (2), the curing temperature is 40-50°C.
[0020] In the second aspect of the present invention, a self-healing high-adhesion low-eutectic solvent gel with self-healing, adhesion, antifreeze, stability and good biocompatibility is provided, which is prepared by the method of the first aspect of the present invention.
[0021] The self-healing high-adhesion eutectic solvent gel of the present invention shows great potential in the preparation of flexible conductive materials, and can be used in the fields of biosensors, medical dressings, drug delivery carriers, tissue engineering scaffolds, and soil protection, such as foldable mobile phones, artificial skin, disease detectors, soft robots, wearable devices and other electronic devices.
[0022] In the third aspect of the present invention, there is provided an application of the self-healing high-adhesion low-eutectic solvent gel according to the second aspect of the present invention, specifically, an application as a flexible conductive material in biosensors, medical dressings, drug delivery carriers, tissue engineering scaffolds, and soil protection.
[0023] Based on the above technical scheme, the concept of the present invention is to use hydrogen bond acceptors and hydrogen bond donors to prepare low eutectic solvents for enhancing the anti-drying and viscosity of gels; and to add starch, nano-chitin, and polyvinyl alcohol to the low eutectic solvents for optimization. Starch is an environmentally friendly natural high molecular weight polysaccharide, and polyvinyl alcohol is a polymer with good hydrophilicity. Its molecular chains all contain a large number of hydroxyl groups and have strong cross-linking ability. Chitin has a large number of hydroxyl groups and acetylamino groups, which are easy to form strong hydrogen bonds within and between molecules. The above components are rich in sources, low in price, non-toxic and non-irritating, and the hydrogels prepared with them as raw materials have good biocompatibility, strong biodegradability, and adjustable physical and chemical properties. The present invention is based on the hydrogen bond network of the low eutectic solvent, so that starch, nano-chitin, polyvinyl alcohol and the advantages of the low eutectic solvent are combined. In addition to the effects of the cross-linking agent and the initiator, it works together with acrylamide or acrylic acid to construct a double-layer network to improve the adhesion and tensile strength of the gel, forming a multifunctional low eutectic solvent gel.
[0024] Compared with the prior art, the present invention has the following advantages and beneficial effects: The invention provides a method for preparing a self-healing high-adhesion low eutectic solvent gel, which has a simple process, is green and environmentally friendly, has a wide and economical source of raw materials, and is conducive to popularization and application.
[0025] The invention provides a self-healing high-adhesion eutectic solvent gel, which has the characteristics of self-healing, adhesion, antifreeze and stability, and is safe, non-toxic and has excellent biocompatibility.
[0026] The present invention provides an application of a self-healing high-adhesion low eutectic solvent gel, which has good application value as a gel material in biosensors, medical dressings, drug delivery carriers, tissue engineering scaffolds, soil protection, etc. DETAILED DESCRIPTION
[0027] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0028] In the following embodiments: Cassava flour (food grade) and ordinary starch (food grade) were purchased from supermarkets, and polyvinyl alcohol (1788) was purchased from Tianjin Huasheng Chemical Reagent Co., Ltd.
[0029] Example 1 The preparation method of the self-healing high-adhesion eutectic solvent gel comprises the following steps: (1) According to the molar ratio of 1:2, 4 g of choline chloride and 5.3 g of glycerol were weighed and added to a conical flask, and the conical flask was placed in an oil bath at 80 °C and stirred for 90 min until a clear and uniform solution was formed to prepare a low eutectic solvent; 2.65 g of acrylamide monomer and 0.01328 g of N,N'-methylenebisacrylamide were added to the low eutectic solvent, and the mixture was stirred at 40 °C for 30 min to mix evenly, cooled to room temperature, and ammonium persulfate solution was added to the conical flask and stirred evenly to obtain a precursor; (2) Weigh 1.5 g of ordinary starch and disperse it in 48.5 g of deionized water to obtain a starch suspension. Stir the suspension at room temperature for 15 min to fully mix it. Adjust its pH to about 5 with a 2 wt.% acetic acid aqueous solution. Then, place it in a magnetic stirrer and stir it at 90 °C for 30 min to gelatinize it. Cool the gelatinized starch suspension to 50 °C, then slowly add the precursor, stir it continuously for 30 min to mix, and then pour it into a mold. Curing is completed at this temperature. After drying, a self-healing high-adhesion low eutectic solvent gel is obtained.
[0030] Example 2 The preparation method of the self-healing high-adhesion eutectic solvent gel comprises the following steps: (1) According to the molar ratio of 1:2, 4 g of choline chloride and 5.3 g of glycerol were weighed and added to a conical flask, and the conical flask was placed in an oil bath at 80 °C and stirred for 90 min until a clear and uniform solution was formed to prepare a low eutectic solvent; 2.65 g of acrylamide monomer and 0.01328 g of N,N'-methylenebisacrylamide were added to the low eutectic solvent, and the mixture was stirred at 40 °C for 30 min to mix evenly, cooled to room temperature, and ammonium persulfate solution was added to the conical flask and stirred evenly to obtain a precursor; (2) Weigh 1.5 g of cassava flour and disperse it in 48.5 g of deionized water to obtain a starch suspension. Stir the suspension at room temperature for 15 min to fully mix it. Adjust its pH to about 5 with a 2 wt.% acetic acid aqueous solution. Then, place it in a magnetic stirrer and stir it at 90 °C for 30 min to gelatinize the amylose. Cool the gelatinized starch suspension to 50 °C, then slowly add the precursor, stir it continuously for 30 min to mix, and then pour it into a mold. Curing is completed at this temperature. After drying, a self-healing high-adhesion low eutectic solvent gel is obtained.
[0031] Example 3 The preparation method of the self-healing high-adhesion eutectic solvent gel comprises the following steps: (1) According to the molar ratio of 1:2, 4 g of choline chloride and 5.3 g of glycerol were weighed and added to a conical flask, and the conical flask was placed in an oil bath at 80 °C and stirred for 90 min until a clear and uniform solution was formed to prepare a low eutectic solvent; 2.65 g of acrylamide monomer and 0.01328 g of N,N'-methylenebisacrylamide were added to the low eutectic solvent, and the mixture was stirred at 40 °C for 30 min to mix evenly, cooled to room temperature, and ammonium persulfate solution was added to the conical flask and stirred evenly to obtain a precursor; (2) Chitosan was used as the raw material, 3 mol / L hydrochloric acid was added at a solid-liquid ratio of 1:20 g / mL, and the mixture was stirred and hydrolyzed in a boiling water bath for 1 h to obtain a nanochitosan suspension. The mixture was washed with water until neutral and then centrifuged. The precipitate was freeze-dried to obtain nanochitosan. 0.15 g of nanochitosan and 1.0 g of ordinary starch were dispersed in 48.5 g of deionized water to obtain a reinforcing agent suspension. The suspension was stirred at room temperature for 15 min to be fully mixed, and then placed in a magnetic stirrer and stirred at 90 °C for 30 min to gelatinize it. The gelatinized reinforcing agent suspension was cooled to 50 °C, and then the precursor was slowly added. The mixture was stirred continuously for 30 min and then poured into a mold. The solidification was completed at this temperature. After drying, a self-healing high-adhesion low eutectic solvent gel was obtained.
[0032] Example 4 The preparation method of the self-healing high-adhesion eutectic solvent gel comprises the following steps: (1) According to the molar ratio of 1:2, 4 g of choline chloride and 5.3 g of glycerol were weighed and added to a conical flask, and the conical flask was placed in an oil bath at 80 °C and stirred for 90 min until a clear and uniform solution was formed to prepare a low eutectic solvent; 2.65 g of acrylamide monomer and 0.01328 g of N,N'-methylenebisacrylamide were added to the low eutectic solvent, and the mixture was stirred at 40 °C for 30 min to mix evenly, cooled to room temperature, and ammonium persulfate solution was added to the conical flask and stirred evenly to obtain a precursor; (2) Using the method of Example 3 to prepare nano-chitosan, 0.15 g of nano-chitosan and 1.5 g of cassava flour were dispersed in 48.5 g of deionized water to obtain a reinforcing agent suspension. The suspension was stirred at room temperature for 15 min to be fully mixed, and its pH was adjusted to about 5 with a 2 wt.% acetic acid aqueous solution. Then, it was placed in a magnetic stirrer and stirred at 90 ° C for 30 min to gelatinize the amylose. The gelatinized reinforcing agent suspension was cooled to 50 ° C, and then the precursor was slowly added. After continuous stirring for 30 min, the mixture was poured into a mold and cured at this temperature. After drying, a self-healing high-adhesion low eutectic solvent gel was obtained.
[0033] Example 5 The preparation method of the self-healing high-adhesion eutectic solvent gel comprises the following steps: (1) According to the molar ratio of 1:2, 4 g of choline chloride and 5.3 g of glycerol were weighed and added to a conical flask, and the conical flask was placed in an oil bath at 80 °C and stirred for 90 min until a clear and uniform solution was formed to prepare a low eutectic solvent; 2.65 g of acrylamide monomer and 0.01328 g of N,N'-methylenebisacrylamide were added to the low eutectic solvent, and the mixture was stirred at 40 °C for 30 min to mix evenly, cooled to room temperature, and ammonium persulfate solution was added to the conical flask and stirred evenly to obtain a precursor; (2) Take 2.5 g of polyvinyl alcohol and disperse it in 13.5 g of deionized water to obtain a polyvinyl alcohol suspension. The suspension is stirred at room temperature for 30 min to be fully mixed. Then, the precursor is slowly added at 50 °C. After continuous stirring for 30 min, the mixture is poured into a mold and cured at this temperature. After drying, a self-healing high-adhesion low-eutectic solvent gel is obtained.
[0034] Example 6 The preparation method of the self-healing high-adhesion eutectic solvent gel comprises the following steps: (1) According to the molar ratio of 1:2, 4 g of choline chloride and 5.5 g of citric acid were weighed and added to a conical flask, and the conical flask was placed in an oil bath at 80 °C and stirred for 90 min until a clear and uniform solution was formed to prepare a low eutectic solvent; 2.65 g of acrylamide monomer and 0.01328 g of N,N'-methylenebisacrylamide were added to the low eutectic solvent, and the mixture was stirred at 40 °C for 30 min to mix evenly, cooled to room temperature, and ammonium persulfate solution was added to the conical flask and stirred evenly to obtain a precursor; (2) Weigh 1.5 g of cassava flour and disperse it in 48.5 g of deionized water to obtain a starch suspension. Stir the suspension at room temperature for 15 min to fully mix it. Adjust its pH to about 5 with a 2 wt.% acetic acid aqueous solution. Then, place it in a magnetic stirrer and stir it at 90 °C for 30 min to gelatinize the amylose. Cool the gelatinized starch suspension to 50 °C, then slowly add the precursor, stir it continuously for 30 min to mix, and then pour it into a mold. Curing is completed at this temperature. After drying, a self-healing high-adhesion low eutectic solvent gel is obtained.
[0035] Example 7 The preparation method of the self-healing high-adhesion eutectic solvent gel comprises the following steps: (1) According to the molar ratio of 1:2, 4 g of choline chloride and 5.5 g of citric acid were weighed and added to a conical flask, and the conical flask was placed in an oil bath at 80 °C and stirred for 90 min until a clear and uniform solution was formed to prepare a low eutectic solvent; 2.65 g of acrylamide monomer and 0.01328 g of N,N'-methylenebisacrylamide were added to the low eutectic solvent, and the mixture was stirred at 40 °C for 30 min to mix evenly, cooled to room temperature, and ammonium persulfate solution was added to the conical flask and stirred evenly to obtain a precursor; (2) Weigh 1.5 g of ordinary starch and disperse it in 48.5 g of deionized water to obtain a starch suspension. Stir the suspension at room temperature for 15 min to fully mix it. Adjust its pH to about 5 with a 2 wt.% acetic acid aqueous solution. Then, place it in a magnetic stirrer and stir it at 90 °C for 30 min to gelatinize the amylose. Cool the gelatinized starch suspension to 50 °C, then slowly add the precursor, stir it continuously for 30 min to mix, and then pour it into a mold. Curing is completed at this temperature. After drying, a self-healing high-adhesion low eutectic solvent gel is obtained.
[0036] Example 8 The preparation method of the self-healing high-adhesion eutectic solvent gel comprises the following steps: (1) According to the molar ratio of 1:2, 4 g of choline chloride and 5.5 g of citric acid were weighed and added to a conical flask, and the conical flask was placed in an oil bath at 80 °C and stirred for 90 min until a clear and uniform solution was formed to prepare a low eutectic solvent; 2.65 g of acrylamide monomer and 0.01328 g of N,N'-methylenebisacrylamide were added to the low eutectic solvent, and the mixture was stirred at 40 °C for 30 min to mix evenly, cooled to room temperature, and ammonium persulfate solution was added to the conical flask and stirred evenly to obtain a precursor; (2) Using the method of Example 3 to prepare nano-chitin, 0.15 g of nano-chitin and 1.0 g of ordinary starch were dispersed in 48.5 g of deionized water to obtain a reinforcing agent suspension. The suspension was stirred at room temperature for 15 min to be fully mixed, and then placed in a magnetic stirrer and stirred at 90 ° C for 30 min to gelatinize it; the gelatinized reinforcing agent suspension was cooled to 50 ° C, and then the precursor was slowly added, and the mixture was stirred continuously for 30 min to mix, and then poured into a mold. The curing was completed at this temperature, and a self-healing high-adhesion low eutectic solvent gel was obtained after drying.
[0037] Example 9 The preparation method of the self-healing high-adhesion eutectic solvent gel comprises the following steps: (1) According to the molar ratio of 1:2, 4 g of choline chloride and 5.5 g of citric acid were weighed and added to a conical flask, and the conical flask was placed in an oil bath at 80 °C and stirred for 90 min until a clear and uniform solution was formed to prepare a low eutectic solvent; 2.65 g of acrylamide monomer and 0.01328 g of N,N'-methylenebisacrylamide were added to the low eutectic solvent, and the mixture was stirred at 40 °C for 30 min to mix evenly, cooled to room temperature, and ammonium persulfate solution was added to the conical flask and stirred evenly to obtain a precursor; (2) Using the method of Example 3 to prepare nano-chitosan, 0.15 g of nano-chitosan and 1.5 g of cassava flour were dispersed in 48.5 g of deionized water to obtain a reinforcing agent suspension, which was stirred at room temperature for 15 min to be fully mixed, and its pH was adjusted to about 5 with a 2 wt.% acetic acid aqueous solution, and then placed in a magnetic stirrer and stirred at 90 ° C for 30 min to gelatinize it; the gelatinized reinforcing agent suspension was cooled to 50 ° C, and then the precursor was slowly added, and the mixture was stirred continuously for 30 min and poured into a mold. The solidification was completed at this temperature, and the self-healing high-adhesion low eutectic solvent gel was obtained after drying.
[0038] Example 10 The preparation method of the self-healing high-adhesion eutectic solvent gel comprises the following steps: (1) According to the molar ratio of 1:2, 4 g of choline chloride and 5.3 g of glycerol were weighed and added to a conical flask, and the conical flask was placed in an oil bath at 80 °C and stirred for 90 min until a clear and uniform solution was formed to prepare a low eutectic solvent; 2.65 g of acrylamide monomer and 0.01328 g of N,N'-methylenebisacrylamide were added to the low eutectic solvent, and the mixture was stirred at 40 °C for 30 min to mix evenly, cooled to room temperature, and ammonium persulfate solution was added to the conical flask and stirred evenly to obtain a precursor; (2) Take 2.5 g of polyvinyl alcohol and disperse it in 13.5 g of deionized water to obtain a polyvinyl alcohol suspension. The suspension is stirred at room temperature for 30 min to be fully mixed. Then, the precursor is slowly added at 50 °C. After continuous stirring for 30 min, the mixture is poured into a mold and cured at this temperature. After drying, a self-healing high-adhesion low-eutectic solvent gel is obtained.
[0039] Embodiment 11 This example studies the performance of the partially self-healing high adhesion eutectic solvent gel prepared above.
[0040] A circular self-healing high-adhesion low eutectic solvent gel sample with a diameter of 20 mm and a thickness of 1.5 mm was attached to the test bench. The spectral test range was 800-200 nm. The transmittance of the sample was characterized and analyzed using a TU-1810 UV-visible spectrophotometer. The test results of the transmittance are shown in Table 1.
[0041] Table 1: Transmittance test results
[0042] The transmittance at 500 nm and 800 nm is used as a representative parameter. The test shows that the transmittance of the self-healing high-adhesion low-eutectic solvent gel in the above wavelength range is greater than 50%, and the gel has good transmittance.
[0043] The self-healing high-adhesion low-eutectic solvent gel was cut into samples with a specification of 40 mm×20 mm×0.3 mm. The tensile properties of the samples were measured using a tensile tester. The test results are shown in Table 2.
[0044] Table 2: Tensile properties test results
[0045] The results in Table 2 show that when a suspension of polyhydroxy reinforcing agent is added to the precursor, the reinforcing material is directly dispersed in the DES hydrogen bond network to undergo free radical polymerization, the interaction between the components and the degree of crosslinking of the hydrogen bond network increase, the rigidity increases after multiple crosslinking, the elongation increases by about 1.5-2.5 times, and the self-healing high adhesion low eutectic solvent gel has good tensile properties.
[0046] In order to study the antifreeze property of the self-healing high-adhesion low eutectic solvent gel, the self-healing high-adhesion low eutectic solvent gel was also cut into samples with a specification of 40 mm×20 mm×0.3 mm and stored at -26 °C for 5 days. Then, the tensile properties of the samples after freezing treatment were measured using a tensile tester under the same test conditions. The test results are shown in Table 3.
[0047] Table 3: Tensile properties test results after freezing treatment
[0048] The results in Table 3 show that the self-healing high-adhesion eutectic solvent gel has good antifreeze properties and can still maintain good tensile properties after freezing treatment.
[0049] In the above embodiments, hydrogen bond acceptors and hydrogen bond donors are used to prepare low eutectic solvents, which enhances the anti-drying and viscosity of the gel; and starch, nano-chitin, and polyvinyl alcohol are added to the low eutectic solvent to complete the optimization. Starch is an environmentally friendly natural high molecular weight polysaccharide, and polyvinyl alcohol is a polymer with good hydrophilicity. Its molecular chains all contain a large number of hydroxyl groups and have strong cross-linking ability. Chitin has a large number of hydroxyl groups and acetylamino groups, which are easy to form strong hydrogen bonds within and between molecules. The above components are rich in sources, low in price, non-toxic and irritating. The hydrogels prepared with them as raw materials have good biocompatibility, strong biodegradability, and adjustable physical and chemical properties. The embodiment is based on the hydrogen bond network of the low eutectic solvent, which combines the advantages of starch, nano-chitin, polyvinyl alcohol and the low eutectic solvent. In addition to the role of the cross-linking agent and initiator, it works together with acrylamide or acrylic acid to construct a double-layer network to improve the adhesion and tensile strength of the gel, forming a multifunctional low eutectic solvent gel.
[0050] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. A method for preparing a self-healing high-adhesion eutectic solvent gel, It is characterized in that The steps include: (1) A low eutectic solvent formed by a hydrogen bond acceptor and a hydrogen bond donor is used as a gel dispersion medium, and a polymerization monomer, a crosslinking agent and an initiator are added thereto to obtain a precursor; (2) adding a suspension of a polyhydroxy reinforcing agent to the precursor, mixing, curing, and drying to obtain a self-healing high-adhesion eutectic solvent gel; Wherein, the polyhydroxy enhancer is selected from at least one of starch, nano-chitin and polyvinyl alcohol.
2. The preparation method according to claim 1, Features: In the step (1), the hydrogen bond acceptor is choline chloride; the hydrogen bond donor is selected from one or two of glycerol, ethylene glycol, urea, and citric acid; and the molar ratio of the hydrogen bond acceptor to the hydrogen bond donor is 1:1-2.
3. The preparation method according to claim 1, It is characterized in that The preparation method of the low eutectic solvent is as follows: a hydrogen bond acceptor and a hydrogen bond donor are mixed at 80-95° C. to obtain a clear solution, and the mixture is cooled to 30-50° C. to obtain a low eutectic solvent.
4. The preparation method according to claim 1, Features: In the step (1), the polymerizable monomer is acrylamide or acrylic acid; and the amount of the polymerizable monomer added accounts for 25%-30% of the mass of the low eutectic solvent.
5. The preparation method according to claim 1, Features: In the step (1), the amount of the cross-linking agent added is 0.5‰-2‰ of the mass of the low eutectic solvent; the amount of the initiator added is 0.6‰-0.8‰ of the mass of the low eutectic solvent.
6. The preparation method according to claim 1, Features: In the step (2), the amount of the polyhydroxy enhancer added is 10%-20% of the mass of the low eutectic solvent.
7. The preparation method according to claim 1, Features: When starch is used as the polyhydroxy enhancer, the starch is gelatinized at 70-90°C in advance and then cooled to 40-50°C, and then its suspension is added to the precursor.
8. The preparation method according to claim 1, Features: In the step (2), the curing temperature is 40-50°C.
9. A self-healing high-adhesion eutectic solvent gel, Features: The method is prepared according to any one of claims 1 to 8.
10. A use of the self-healing high-adhesion eutectic solvent gel as claimed in claim 9, Features: Applications as flexible conductive materials in biosensors, medical dressings, drug delivery carriers, tissue engineering scaffolds, and soil protection.
Citation Information
Patent Citations
Method for preparing conductive polysaccharide compound hydrogel by adopting front-end polymerization of polysaccharide eutectic solvent mixture solution
CN112876611A
Self-healing, anti-freezing and self-adhesive conductive ion hydrogel with birefringence characteristic as well as preparation method and application of self-healing, anti-freezing and self-adhesive conductive ion hydrogel
CN115368509A
Preparation method and application of high-freezing-resistance dual-network eutectic gel
CN117050342A
Preparation method of eutectic gel with adjustable mechanical properties
CN117487059A
Cited By
Preparation method and application of eutectic gel
CN119978685A
Phase-change-controllable eutectic gel as well as preparation method and application thereof
CN121592152A