Waste polystyrene-based water reducing agent and preparation method thereof

Through peroxide degradation, carboxy monomer grafting, sulfonation and esterification, polyethylene glycol branching, and ultrasonic degradation, the problem of excessive molecular weight when used polystyrene is converted into concrete water reducing agent is solved. It achieves efficient water reduction and fluid retention rates, and realizes efficient reuse of waste polystyrene.

CN118909196APending Publication Date: 2024-11-08JIANGMEN POLYTECHNIC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411136583.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, the method of converting waste polystyrene into concrete water reducing agent leads to excessive molecular weight, low water reduction rate, and the use of a sodium oxide catalyst will consume hydrogen ions, affecting the sulfonation reaction.

Method used

Peroxide degradation and carboxy monomer grafting, sulfonation and esterification grafting polyethylene glycol branched chains, and degradation through ultrasonic action, waste polystyrene-based concrete water reducing agent with lower molecular weight was prepared.

Benefits of technology

A high water reduction rate and fluid retention rate are achieved, excellent performance, and energy circulation is realized by efficient reuse of waste polystyrene.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004999596400000041
    Figure BDA0004999596400000041
  • Figure BDA0004999596400000121
    Figure BDA0004999596400000121
Patent Text Reader

Abstract

The invention provides a waste polystyrene-based water reducing agent and a preparation method thereof, and relates to the technical field of polymer waste treatment. The waste polystyrene-based concrete water reducing agent is prepared from the following components in parts by weight: 9 to 11 parts of waste polystyrene, 30 to 40 parts of solvent, 0.1 to 0.3 part of initiator, 3 to 4 parts of maleic anhydride, 16 to 20 parts of concentrated sulfuric acid, 0.1 to 0.3 part of phosphorus pentoxide and 5 to 8 parts of polyethylene glycol. According to the method, peroxide degradation and carboxyl introduction are carried out at the same time, polyethylene glycol long-chain branch introduction and sulfonation reaction are carried out at the same time, and the molecular weight of the product is further reduced through ultrasonic waves, so that a water-soluble high-molecular product with low molecular weight and carboxyl, polyethylene glycol long-chain branch and sulfonate radical groups is obtained; according to the waste polystyrene-based water reducing agent provided by the invention, the water reducing rate and the fluidity retention rate are relatively high, and the performance is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer waste treatment, and in particular to a waste polystyrene-based water reducer and a preparation method thereof. Background Art

[0002] Polystyrene is a plastic widely used in packaging materials. Due to its difficulty in degradation, it causes environmental pollution after being discarded. In the prior art, there are few methods for recycling polystyrene, and the effect is not good. Therefore, it is of great practical significance to develop a method for converting waste polystyrene into valuable chemical products.

[0003] Concrete water reducer is an important admixture in the concrete industry. It can significantly improve the fluidity and working performance of concrete, reduce water consumption, and thus improve the strength and durability of concrete. At present, concrete water reducer is mainly made by chemical synthesis, with high raw material cost and complex process. Therefore, converting waste polystyrene into concrete water reducer can not only reduce environmental pollution, but also expand the source of raw materials for concrete water reducer.

[0004] The existing method of converting waste polystyrene into concrete water reducer is mainly to prepare water-soluble polymer by sulfonating and neutralizing polystyrene. The molecular structure of this water reducer is similar to that of naphthalene water reducer. For example, the preparation method provided by Chinese patent ZL99117093.8 is to dissolve or swell polystyrene in toluene, dichloroethane or xylene, use chlorosulfonic acid or sulfuric acid with a weight concentration of 50%-99% as a sulfonating agent to react for 3-5 hours, and distill and recover the solvent; add water, dissolve the sulfonated polystyrene in water, and then neutralize with calcium hydroxide, calcium oxide or lime, and filter it into a stable cement water reducer solution. However, the water reducer prepared by this method has a high molecular weight, and the dominant functional group is only sulfonate, which is relatively simple, so the water reduction rate is not high and the slump retention is poor.

[0005] In order to solve the problem of too high molecular weight, Chinese patent ZL201210569607.2 heats and melts waste polystyrene plastic before sulfonation, and then adds sodium oxide to degrade it at high temperature. Although this method can lower the molecular weight, the use of sodium oxide as a catalyst will inevitably react with the concentrated sulfuric acid used in sulfonation to consume hydrogen ions, reduce the concentration of concentrated sulfuric acid, which is not conducive to sulfonation, and increase the by-product of sodium sulfate. Summary of the invention

[0006] The purpose of the present application is to provide a waste polystyrene-based concrete water reducer, which has a high water reduction rate and fluidity retention rate.

[0007] Another object of the present application is to provide a method for preparing a waste polystyrene-based concrete water reducer, wherein the water reducer is prepared by peroxide degradation and carboxyl monomer grafting, sulfonation and esterification grafting of polyethylene glycol side chains, and ultrasonication of solution molecular chain degradation.

[0008] In order to solve the above technical problems, the technical solution adopted in this application is:

[0009] On the one hand, the present application provides a waste polystyrene-based concrete water reducer, the raw materials of which include the following components in parts by weight:

[0010] 9-11 parts of waste polystyrene, 30-40 parts of solvent, 0.1-0.3 parts of initiator, 3-4 parts of maleic anhydride, 16-20 parts of concentrated sulfuric acid, 0.1-0.3 parts of phosphorus pentoxide and 5-8 parts of polyethylene glycol.

[0011] On the other hand, the present application provides a method for preparing a waste polystyrene-based concrete water reducer, comprising the following steps:

[0012] S1, taking waste polystyrene particles and a solvent, mixing and dissolving them, adding maleic anhydride, and heating to form a solution I;

[0013] S2, mixing the initiator and the solvent to prepare solution II, adding solution II to solution I, stirring and reacting to obtain solution III;

[0014] S3, adding phosphorus pentoxide and polyethylene glycol to solution III, adding concentrated sulfuric acid under stirring, reacting, and recovering the solvent after the reaction to obtain a reaction solution;

[0015] S4, cooling the reaction solution to room temperature, adjusting the pH to 6-9, adding water to adjust the concentration to 20-30%, and obtaining a reaction product;

[0016] S5. Subjecting the reaction product to ultrasonic irradiation to obtain the waste polystyrene-based concrete water reducing agent.

[0017] The reaction principle of this application includes:

[0018] 1. Dissolve waste polystyrene in a solvent, heat it to 75-80°C, and then add maleic anhydride and initiator, which will produce the following reaction:

[0019] 1) Initiator decomposition: Taking benzoyl peroxide as an example, it will decompose at 75-80°C to generate free radicals, causing BPO to decompose into two benzoyloxy free radicals. The reaction formula is as follows:

[0020] (C6H5CO)2O2→2C6H5CO·

[0021] 2) Free radicalization of polystyrene chains: The free radicals generated by the decomposition of the initiator can attack the carbon atoms on the polystyrene chain to form polystyrene free radicals; benzoyl peroxide decomposes at high temperature to produce free radicals, which attack the polystyrene chain, causing the polymer chain to break and generate low molecular weight degradation products.

[0022] 3) Copolymerization of maleic anhydride: Maleic anhydride can react with polystyrene free radicals to form copolymers. Maleic anhydride, as a comonomer, can react with polystyrene free radicals and insert into the polystyrene chain to form a copolymer containing maleic anhydride groups:

[0023] PS·+MA→PS-MA

[0024] 4) Further reaction: Continuing free radical reaction may cause more maleic anhydride to combine with polystyrene chains, or cause polystyrene chains to react with other segments to form a complex polymer structure:

[0025] PS-MA·+PS·→PS-MA-PS

[0026] 2. After the above reaction is completed, adding concentrated sulfuric acid (H2SO4) and polyethylene glycol (PEG) will trigger the following reactions and results:

[0027] 1) Esterification reaction of maleic anhydride: Concentrated sulfuric acid, as a strong acid catalyst, can catalyze the esterification reaction of maleic anhydride and polyethylene glycol; the anhydride group in maleic anhydride can react with the hydroxyl group in polyethylene glycol to form an ester bond to generate polyethylene glycol side chains:

[0028]

[0029] 2) Sulfonation of polystyrene by sulfuric acid: concentrated sulfuric acid produces a sulfonation reaction on polystyrene, causing the benzene rings on the polystyrene chain to undergo sulfonation and generate sulfonic acid groups. The presence of phosphorus pentoxide acts as a catalytic agent for sulfonation:

[0030] PS+H2SO4→PS-SO3H+H2O

[0031] 3. Ultrasonic degradation:

[0032] Ultrasonic irradiation can produce cavitation, which is the formation and collapse of small bubbles in the liquid. When these bubbles collapse, they will generate high temperature and pressure, which will break the polymer chains and cause the molecular weight of polystyrene to decrease, that is, degradation.

[0033] Compared with the prior art, the embodiments of the present application have at least the following advantages or beneficial effects:

[0034] 1. The present application obtains a water-soluble polymer product with a low molecular weight having carboxyl groups, long polyethylene glycol branches, and sulfonate groups by simultaneously carrying out peroxide degradation and carboxyl group introduction, simultaneously carrying out polyethylene glycol long chain branching and sulfonation reaction, and further reducing the product molecular weight by ultrasound, namely, the waste polystyrene-based water reducer in the present application. The water reducer achieves a high water reduction rate and fluidity retention rate and has excellent performance.

[0035] 2. This application provides an efficient method for recycling waste polystyrene, achieving energy recycling, and has broad application prospects and market value. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0037] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to specific embodiments.

[0038] A waste polystyrene-based concrete water reducing agent, the raw materials of which include the following components in parts by weight:

[0039] 9-11 parts of waste polystyrene, 30-40 parts of solvent, 0.1-0.3 parts of initiator, 3-4 parts of maleic anhydride, 16-20 parts of concentrated sulfuric acid, 0.1-0.3 parts of phosphorus pentoxide and 5-8 parts of polyethylene glycol.

[0040] In some embodiments of the present application, the solvent is cyclohexane and / or ethylene dichloride.

[0041] In some embodiments of the present application, the initiator is dibenzoyl peroxide and / or dodecyl peroxide.

[0042] In some embodiments of the present application, the above-mentioned polyethylene glycol is polyethylene glycol 400 and / or polyethylene glycol 600.

[0043] A method for preparing a waste polystyrene-based concrete water reducer comprises the following steps:

[0044] S1, taking waste polystyrene particles and a solvent, mixing and dissolving them, adding maleic anhydride, and heating to form a solution I;

[0045] S2, mixing the initiator and the solvent to prepare solution II, adding solution II to solution I, stirring and reacting to obtain solution III;

[0046] S3, adding phosphorus pentoxide and polyethylene glycol to solution III, adding concentrated sulfuric acid under stirring, reacting, and recovering the solvent after the reaction to obtain a reaction solution;

[0047] S4, cooling the reaction solution to room temperature, adjusting the pH to 6-9, adding water to adjust the concentration to 20-30%, and obtaining a reaction product;

[0048] S5. Subjecting the reaction product to ultrasonic irradiation to obtain the waste polystyrene-based concrete water reducing agent.

[0049] In some embodiments of the present application, the heating temperature in the above step S1 is 75-80°C.

[0050] In some embodiments of the present application, the concentration of the initiator in solution II in the above step S2 is 10%, and solution II is added to solution I by dropwise addition, and the stirring reaction time is 2-3 hours.

[0051] In some embodiments of the present application, in the above step S3, concentrated sulfuric acid is added dropwise, the reaction temperature is 70-80° C., and the reaction time is 3-4 h.

[0052] In some embodiments of the present application, a 30% sodium hydroxide solution is used to adjust the pH in the above step S4.

[0053] In some embodiments of the present application, the ultrasonic irradiation time in the above step S5 is 0.5h.

[0054] The features and performance of the present application are further described in detail below in conjunction with the embodiments.

[0055] Example 1

[0056] A waste polystyrene-based water reducer is prepared by the following process:

[0057] S1. Take 10 g of waste polystyrene particles and 28 g of cyclohexane into a three-necked bottle, stir and mix to form a solution, then add 3 g of maleic anhydride, heat to 80° C., and obtain solution I.

[0058] S2. Take 0.2 g of benzoyl peroxide and add it to 1.8 g of cyclohexane to prepare a solution II with a concentration of 10%. Add the solution II dropwise into a three-necked flask within 1 h, stir and react for 2 h to obtain a solution III.

[0059] S3, first add 0.2g of phosphorus pentoxide and 4g of polyethylene glycol 400 to solution III, and under stirring, dropwise add 18mL of concentrated sulfuric acid within 1h, control the reaction temperature at 80°C, and the reaction time is 3h. After the reaction is completed, the solvent is recovered by vacuum distillation to obtain a reaction solution.

[0060] S4. Cool the reaction solution to room temperature, slowly add 30% sodium hydroxide solution to neutralize to a pH value of 6-9, and add distilled water to prepare a reaction product with a concentration of 25%.

[0061] S5. Finally, the reaction product is poured into an ultrasonic reactor and ultrasonically irradiated for 0.5 h in a tap water circulating water bath with an irradiation power (expressed as the power applied to the variable-radius rod) of 400 W to obtain the finished product of the waste polystyrene-based concrete water-reducing agent of this embodiment.

[0062] Example 2

[0063] A waste polystyrene-based water reducer is prepared by the following process:

[0064] S1. Take 10 g of waste polystyrene particles and 35 g of ethylene dichloride into a three-necked bottle, stir and mix to form a solution, then add 4 g of maleic anhydride, heat to 75° C., and obtain solution I.

[0065] S2. Take 0.3 g of dodecyl oxide and add it to 2.7 g of dichloroethane to prepare a solution II with a concentration of 10%. Add solution II dropwise into a three-necked flask within 1 hour, stir and react for 2.5 hours to obtain solution III.

[0066] S3, first add 0.1g of phosphorus pentoxide and 4g of polyethylene glycol 600 to solution III, and under stirring, dropwise add 16mL of concentrated sulfuric acid within 1h, control the reaction temperature at 80°C, and the reaction time is 3h. After the reaction is completed, the solvent is recovered by vacuum distillation to obtain a reaction solution.

[0067] S4. Cool the reaction solution to room temperature, slowly add 30% sodium hydroxide solution to neutralize to a pH value of 6-9, and add distilled water to prepare a reaction product with a concentration of 20%.

[0068] S5. Finally, the reaction product is poured into an ultrasonic reactor and ultrasonically irradiated for 0.5 h in a tap water circulating water bath with an irradiation power (expressed as the power applied to the variable-radius rod) of 400 W to obtain the finished product of the waste polystyrene-based concrete water-reducing agent of this embodiment.

[0069] Example 3

[0070] A waste polystyrene-based water reducer is prepared by the following process:

[0071] S1. Take 10 g of waste polystyrene particles and 37 g of ethylene dichloride into a three-necked bottle, stir and mix to form a solution, then add 5 g of maleic anhydride, heat to 75° C., and obtain solution I.

[0072] S2. Take 0.3 g of dodecyl oxide and add it to 2.7 g of dichloroethane to prepare a solution II with a concentration of 10%. Add the solution II dropwise into a three-necked flask within 1 hour, stir and react for 2 hours to obtain a solution III.

[0073] S3, first add 0.3g of phosphorus pentoxide and 6g of polyethylene glycol 600 to solution III, and under stirring, dropwise add 20mL of concentrated sulfuric acid within 1h, control the reaction temperature at 80°C, and the reaction time is 3.5h. After the reaction is completed, the solvent is recovered by vacuum distillation to obtain a reaction solution.

[0074] S4. Cool the reaction solution to room temperature, slowly add 30% sodium hydroxide solution to neutralize to a pH value of 6-9, and add distilled water to prepare a reaction product with a concentration of 20%.

[0075] S5. Finally, the reaction product is poured into an ultrasonic reactor and ultrasonically irradiated for 0.5 h in a tap water circulating water bath with an irradiation power (expressed as the power applied to the variable-radius rod) of 400 W to obtain the finished product of the waste polystyrene-based concrete water-reducing agent of this embodiment.

[0076] Example 4

[0077] A waste polystyrene-based water reducer is prepared by the following process:

[0078] S1. Take 10 g of waste polystyrene particles and 28 g of cyclohexane into a three-necked bottle, stir and mix to form a solution, then add 3 g of maleic anhydride, heat to 80° C., and obtain solution I.

[0079] S2. Take 0.2 g of benzoyl peroxide and add it to 1.8 g of cyclohexane to prepare a solution II with a concentration of 10%. Add the solution II dropwise into a three-necked flask within 1 h, stir and react for 2 h to obtain a solution III.

[0080] S3, first add 0.2g of phosphorus pentoxide and 4g of polyethylene glycol 400 to solution III, and under stirring, dropwise add 18mL of concentrated sulfuric acid within 1h, control the reaction temperature at 80°C, and the reaction time is 3h. After the reaction is completed, the solvent is recovered by vacuum distillation to obtain a reaction solution.

[0081] S4. Cool the reaction solution to room temperature, slowly add 30% sodium hydroxide solution to neutralize to a pH value of 6-9, and add distilled water to prepare a reaction product with a concentration of 25%.

[0082] S5. Finally, the reaction product is poured into an ultrasonic reactor and ultrasonically irradiated for 0.5 h in a tap water circulating water bath with an irradiation power (expressed as the power applied to the variable-radius rod) of 500 W to obtain the finished product of the waste polystyrene-based concrete water-reducing agent of this embodiment.

[0083] Example 5

[0084] A waste polystyrene-based water reducer is prepared by the following process:

[0085] S1. Take 10 g of waste polystyrene particles and 28 g of cyclohexane into a three-necked bottle, stir and mix to form a solution, then add 3 g of maleic anhydride, heat to 80° C., and obtain solution I.

[0086] S2. Take 0.2 g of benzoyl peroxide and add it to 1.8 g of cyclohexane to prepare a solution II with a concentration of 10%. Add the solution II dropwise into a three-necked flask within 1 h, stir and react for 2 h to obtain a solution III.

[0087] S3, first add 0.2g of phosphorus pentoxide and 4g of polyethylene glycol 400 to solution III, and under stirring, dropwise add 18mL of concentrated sulfuric acid within 1h, control the reaction temperature at 80°C, and the reaction time is 3h. After the reaction is completed, the solvent is recovered by vacuum distillation to obtain a reaction solution.

[0088] S4. Cool the reaction solution to room temperature, slowly add 30% sodium hydroxide solution to neutralize to a pH value of 6-9, and add distilled water to prepare a reaction product with a concentration of 25%.

[0089] S5. Finally, the reaction product is poured into an ultrasonic reactor and ultrasonically irradiated for 0.5 h in a tap water circulating water bath with an irradiation power (expressed as the power applied to the variable-radius rod) of 300 W to obtain the finished product of the waste polystyrene-based concrete water-reducing agent of this embodiment.

[0090] Comparative Example 1

[0091] The difference between this comparative example and Example 1 is that there is no initiator in this comparative example.

[0092] Comparative Example 2

[0093] The difference between this comparative example and Example 1 is that there is no polyethylene glycol in this comparative example.

[0094] Comparative Example 3

[0095] The difference between this comparative example and Example 1 is that there is no ultrasonic irradiation treatment in this comparative example (ie, the reaction product obtained after step S4 is recorded as the waste polystyrene-based water-reducing agent product).

[0096] Comparative Example 4

[0097] The difference between this comparative example and Example 1 is that the conditions of ultrasonic irradiation treatment in this comparative example are: ultrasonic irradiation for 0.5 h in a tap water circulating water bath, and the irradiation power (expressed as the power applied to the variable-radius rod) is 50W.

[0098] Comparative Example 5

[0099] The difference between this comparative example and Example 1 is that in this comparative example, maleic anhydride is replaced by acrylic acid.

[0100] Experimental example

[0101] In this experimental example, the products prepared in Examples 1-5 and Comparative Examples 1-5 were tested according to the Test Method for Homogeneity of Concrete Admixtures GB / T 8077-2023. The test results are shown in Table 1.

[0102] Table 1

[0103]

[0104] As can be seen from Table 1, the water reducers prepared in Examples 1-5 have excellent and stable performance, and the product performance of Comparative Examples 1-5 is reduced compared with that of Example 1, indicating that the present application generates polyethylene glycol side chains by introducing carboxyl groups, anhydride groups in maleic anhydride and hydroxyl groups in polyethylene glycol to react to form ester bonds; and ultrasonic degradation is used to reduce the molecular weight to obtain waste polystyrene-based water reducers, which have an irreplaceable role in achieving a higher water reduction rate and fluidity retention rate.

[0105] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present application.

Claims

1. A waste polystyrene-based concrete water reducer, characterized in that: The raw materials for its preparation include the following components in parts by weight: 9-11 parts of waste polystyrene, 30-40 parts of solvent, 0.1-0.3 parts of initiator, 3-4 parts of maleic anhydride, 16-20 parts of concentrated sulfuric acid, 0.1-0.3 parts of phosphorus pentoxide and 5-8 parts of polyethylene glycol.

2. A waste polystyrene-based concrete water reducer according to claim 1, characterized in that: The solvent is cyclohexane and / or ethylene dichloride.

3. The waste polystyrene-based concrete water reducing agent according to claim 1, characterized in that: The initiator is dibenzoyl peroxide and / or dodecyl peroxide.

4. The waste polystyrene-based concrete water reducer according to claim 1, characterized in that: The polyethylene glycol is polyethylene glycol 400 and / or polyethylene glycol 600.

5. A method for preparing the waste polystyrene-based concrete water reducer according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1, taking waste polystyrene particles and a solvent, mixing and dissolving them, adding maleic anhydride, and heating to form a solution I; S2, mixing the initiator and the solvent to prepare solution II, adding solution II to solution I, stirring and reacting to obtain solution III; S3, adding phosphorus pentoxide and polyethylene glycol to solution III, adding concentrated sulfuric acid under stirring, reacting, and recovering the solvent after the reaction to obtain a reaction solution; S4, cooling the reaction solution to room temperature, adjusting the pH to 6-9, adding water to adjust the concentration to 20-30%, and obtaining a reaction product; S5. Subjecting the reaction product to ultrasonic irradiation to obtain the waste polystyrene-based concrete water reducing agent.

6. The method for preparing a waste polystyrene-based concrete water reducing agent according to claim 5, characterized in that: The heating temperature in the step S1 is 75-80°C.

7. The method for preparing a waste polystyrene-based concrete water reducing agent according to claim 5, characterized in that: In step S2, the concentration of the initiator in solution II is 10%, and solution II is added to solution I by dropwise addition, and the stirring reaction time is 2-3 hours.

8. The method for preparing a waste polystyrene-based concrete water reducing agent according to claim 5, characterized in that: In the step S3, concentrated sulfuric acid is added dropwise, the reaction temperature is 70-80° C., and the reaction time is 3-4 h.

9. The method for preparing a waste polystyrene-based concrete water reducing agent according to claim 5, characterized in that: In the step S4, a 30% sodium hydroxide solution is used to adjust the pH.

10. The method for preparing a waste polystyrene-based concrete water reducing agent according to claim 5, characterized in that: The ultrasonic irradiation time in step S5 is 0.5h, and the ultrasonic power is 300-500W.