Preparation method and application of protein marine polysaccharide hydrogel dressing with conductivity
By using conductive hydrogels composed of proteins and marine polysaccharides, combined with PEDOT:PSS and Ru-TA nanorods, the problem that traditional dressings cannot regulate the wound healing environment is solved, achieving efficient wound healing and antioxidant effects without the need for Initiators and toxic materials.
Patent Information
- Application Number
- CN202410971374.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
Smart Images

Figure CN118909271A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of biomaterials, and in particular to a preparation method and application of a conductive protein marine polysaccharide hydrogel dressing. Background Art
[0002] Skin wounds, especially chronic wounds, are difficult to heal, which seriously affects the normal life of patients and increases the burden on the social medical system. Traditional wound dressings can only protect wounds and cannot regulate the healing environment of wounds. Hydrogel, as a three-dimensional porous material with excellent hydrophilicity and biocompatibility, is regarded as one of the candidates for ideal wound dressings. It can maintain a moist environment at the wound site, and its porous structure is similar to the extracellular matrix and can support cell growth. In addition, hydrogels contain functional particles that are easy to load drugs or other functional particles, thereby improving cell proliferation and the healing effect of wound sites.
[0003] In terms of material selection for hydrogels, most of the hydrogel materials currently under study require the addition of initiators to initiate polymerization to form a solidified gel, such as photoinitiators and thermal initiators. However, the initiator itself has certain toxicity and will reduce the biocompatibility of the hydrogel material. After the egg white in the egg is heated, the protein in it will solidify into a solid. Inspired by this, preparing a protein aqueous solution and heating it can quickly obtain a protein hydrogel without adding an initiator during the process. In addition to protein, polysaccharides are also one of the most widely used natural hydrogel materials. Among them, marine polysaccharides are abundant and can be extracted from algae, fungi, and crustaceans. Polysaccharides derived from marine organisms have biological activities and functionality that are lacking in terrestrial polysaccharides, such as anticoagulant, antioxidant, antithrombotic and antitumor properties.
[0004] In addition to constructing the basic scaffold material of the hydrogel, the regulation of the properties of the hydrogel itself is the key to improving its function. Slow healing of wounds, especially chronic wounds, can cause great pain to patients, and traditional dressings cannot regulate the healing process of wounds through external factors. Exogenous electrical stimulation (ES) can accelerate the healing process of wounds as a way to simulate the endogenous electric field of the wound. As a flexible material, hydrogel is suitable as a medium for conducting electric fields. Hydrogel materials with suitable electrical conductivity can be constructed as dressings combined with electrical stimulation to treat wounds. In addition, ROS generated in the wound can cause oxidative stress and inflammation at the wound site. Therefore, wound dressings also need to have the ability to remove excess ROS to regulate the microenvironment at the wound site. In order to eliminate excess ROS, nanomaterials with strong antioxidant properties can be loaded in the hydrogel. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a method for preparing and applying a protein marine polysaccharide hydrogel dressing with conductivity. The hydrogel dressing does not need to be solidified by an initiator, and is composed of a basic hydrogel of natural protein and marine polysaccharide. The material is prepared by utilizing the property that the protein solution can be directly solidified after heating. At the same time, an appropriate amount of PEDOT:PSS conductive polymer is added to the hydrogel to give the hydrogel electrical activity. In addition, Ru-TA nanorods with strong ROS scavenging ability are prepared and loaded into the hydrogel as an antioxidant material.
[0006] To achieve the above purpose, the technical solution designed by the present invention is as follows:
[0007] The present invention provides a method for preparing a conductive protein marine polysaccharide hydrogel dressing, comprising the following steps:
[0008] (1) preparing a poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) aqueous solution (PEDOT:PSS aqueous solution), a 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride solution (EDC solution), and an N-hydroxysuccinimide solution (NHS solution);
[0009] (2) adding bovine serum albumin (BSA), marine polysaccharide and Ru-TA nanorods to a poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) aqueous solution and stirring to obtain a composite solution;
[0010] (3) Add 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride solution and N-hydroxysuccinimide solution to the composite solution, stir rapidly to obtain a mixed solution, pour the mixed solution into a mold, place the mold in a water bath and heat at high temperature, and the solution solidifies into a hydrogel to obtain a conductive protein marine polysaccharide hydrogel dressing.
[0011] Further, in the step 1), the concentration of the poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) aqueous solution is 0.22wt% to 0.65wt%; the concentration of the 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride solution is 1g / mL; the concentration of the N-hydroxysuccinimide solution is 1g / mL;
[0012] Furthermore, in the step 1), the volume ratio of the poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) aqueous solution, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride solution and N-hydroxysuccinimide solution is 1:0.01-0.02:0.01-0.02.
[0013] Furthermore, in the step 1), the volume ratio of the poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) aqueous solution, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride solution and N-hydroxysuccinimide solution is 1:0.015:0.015.
[0014] Furthermore, in the step 2), the marine polysaccharide is chitosan or fucoidan; the mass ratio of bovine serum albumin, marine polysaccharide and Ru-TA nanorods is 1:0.05-0.5:0.005-0.03; and 0.17 g of bovine serum albumin is added to each milliliter of poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) aqueous solution.
[0015] Furthermore, in the step 2), the concentration of the poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) aqueous solution is 0.43wt%; 0.17g of bovine serum albumin, 0.034g of fucoidan and 0.0034g of Ru-TA nanorods are added to each milliliter of the poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) aqueous solution.
[0016] Furthermore, in the step 2), the high temperature condition is 80° C. and the heating time is 3 min.
[0017] Furthermore, the preparation method of the Ru-TA nanorods is as follows:
[0018] (1) Poloxamer is dissolved in an ethanol solution and stirred until completely dissolved, then aqueous ammonia is added to the solution to adjust the pH to 9 to 12, then tannic acid is added to the solution and stirred, and ruthenium trichloride is added and stirred;
[0019] (2) transferring the solution to a hydrothermal reactor, placing the hydrothermal reactor in an oven for heating, reacting, waiting for the reactor to cool naturally to room temperature, and centrifuging;
[0020] (3) removing the supernatant from the centrifuge tube, adding deionized water for vortex washing, and then centrifuging again to remove the supernatant. Repeating the above washing and centrifugation steps for 3 times, the final precipitate product is freeze-dried to obtain Ru-TA nanorod powder.
[0021] Furthermore, in the step 1), the mass ratio of poloxamer, tannic acid and ruthenium trichloride is 1:0.5-2:0.1-1; the volume fraction of the ethanol solution is 8%-25%; and 0.0037g of poloxamer is added to each milliliter of ethanol solution.
[0022] Furthermore, in step 1), the volume fraction of the ethanol solution is 13.04%; 0.0037g of poloxamer, 0.0056g of tannic acid and 0.0026g of ruthenium trichloride are added to each milliliter of ethanol solution.
[0023] Furthermore, in the step 1), add aqueous ammonia and stir for 1 hour; add tannic acid and stir for 24 hours; add ruthenium trichloride and stir for 24 hours.
[0024] Furthermore, in the step 2), the heating temperature is 100° C. and the reaction time is 24 hours.
[0025] The present invention also provides an application of the conductive protein marine polysaccharide hydrogel dressing prepared by the preparation method in the preparation of products for improving cell proliferation and wound healing.
[0026] Principle of the present invention:
[0027] 1. Traditional metal-polyphenol networks are mostly used to modify the surface of materials in the form of coatings, and this bonding method is unstable. The hydrophilic metal-polyphenol coating formed on the surface of the material is easy to fall off when washing with water and ultrasonic materials. In the present invention, a hydrothermal synthesis method is used to prepare Ru-TA nanorods that can exist stably, and the nanorods are loaded in a hydrogel, which solves the problem that the metal-polyphenol network material cannot be stably combined with other materials.
[0028] 2. The protein used in the present invention is BSA, which is a cell culture medium additive that can promote cell growth and survival. Inspired by the phenomenon that protein in egg white coagulates when heated, the BSA protein is directly heated to construct a hydrogel.
[0029] 3. The marine polysaccharides in the hydrogel material of the present invention are rich in sources, and the marine polysaccharides can support the proliferation of wound cells, and also have special biological activities that terrestrial polysaccharides do not have, such as the anti-inflammatory ability of fucoidan.
[0030] 4. The hydrogel of the present invention adds PEDOT:PSS with good water solubility, high conductivity and low toxicity to improve the conductivity of the hydrogel. The prepared hydrogel is used as an electroactive medium to conduct an external electric field to perform electrical stimulation treatment on the wound, thereby accelerating the wound healing process.
[0031] Beneficial effects of the present invention:
[0032] The present invention uses a hydrothermal synthesis method to prepare Ru-TA nanorods that can exist stably, and loads them in a hydrogel, thereby solving the problem that the metal-polyphenol network material cannot be stably combined with other materials. The conductive protein marine polysaccharide hydrogel dressing prepared by the present invention does not need to add an initiator during the preparation process, the preparation method is simple and pollution-free, and no toxic initiator is added, and the hydrogel has excellent biocompatibility. The hydrogel of the present invention adds PEDOT:PSS with good water solubility, high conductivity and low toxicity to improve the conductivity of the hydrogel. The prepared hydrogel is used as an electroactive medium to conduct an external electric field to electrically stimulate the wound for treatment, thereby accelerating the wound healing process. At the same time, the Ru-TA in the hydrogel can remove excess ROS in the wound and maintain the microenvironmental homeostasis of the wound site. Reduce the inflammatory response at the wound site. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 Optical microscope image of Ru-TA nanorods;
[0034] Figure 2 TEM image of Ru-TA nanorods;
[0035] Figure 3 FTIR image of BPPR hydrogel;
[0036] Figure 4 is the conductivity value diagram of the hydrogel;
[0037] Figure 5 To remove H from the hydrogel 2 O 2 Then the scanning curve diagram at 300-700nm wavelength;
[0038] Figure 6 To remove H from the hydrogel 2 O 2 Clearance plot of
[0039] Figure 7 The figure shows the cell proliferation results under conditions of no electrical stimulation and electrical stimulation;
[0040] Figure 8 Fluorescence images of cells stained with DCFH-DA and DAPI;
[0041] Fig. 9 Experimental images of hydrogels treating rat skin wounds 7 days after treatment without electrical stimulation and with electrical stimulation;
[0042] Fig.10 The wound area of rat skin wounds treated with hydrogels under no electrical stimulation and electrical stimulation conditions for 7 days. DETAILED DESCRIPTION
[0043] The present invention is further described in detail below in conjunction with specific embodiments so that those skilled in the art can understand.
[0044] Example 1
[0045] 1. Preparation of Ru-TA Nanorods 1
[0046] (1) F127 was dissolved in a 9.09% ethanol solution (ethanol to water volume ratio of 1:10) and stirred until completely dissolved. Then, 28% ammonia water was added to the mixed solvent, the pH was adjusted to 9-12, the volume ratio of ammonia water to the mixed solvent was 1:540, and stirred for 1 hour. Tannic acid was then added to the solution, stirred for 24 hours, and RuCl was added. 3 ·3H 2 O, stirred for 24 h, 0.0037 g F127, 0.00185 g tannic acid and 0.00037 g RuCl were added per ml of ethanol solution. 3 ·3H 2 O.
[0047] (2) The solution was transferred to a hydrothermal reactor, which was placed in an oven and heated to 100°C for 24 hours. After the reactor was cooled to room temperature naturally, the solution in the reactor was transferred to a centrifuge tube and centrifuged at 8000 rpm for 10 minutes.
[0048] (3) removing the supernatant from the centrifuge tube, adding deionized water for vortex washing, and then centrifuging again to remove the supernatant. Repeating the above washing and centrifugation steps for 3 times, freeze-drying the final precipitate to obtain a powder, which is Ru-TA nanorods 1.
[0049] 2. Preparation of Conductive Protein Marine Polysaccharide Hydrogel Dressing 1
[0050] (1) A 0.22 wt % PEDOT:PSS aqueous solution, a 1 g / mL EDC solution and a 1 g / mL NHS solution were prepared, and the volume ratio of the PEDOT:PSS aqueous solution, the EDC solution and the NHS solution was 1:0.01:0.01.
[0051] (2) BSA, chitosan and Ru-TA nanorods 1 were added to a 0.22 wt % PEDOT:PSS aqueous solution and stirred for 30 min. 0.17 g BSA, 0.0085 g chitosan and 0.00085 g Ru-TA nanorods 1 were added to each ml of the PEDOT:PSS aqueous solution.
[0052] (3) Then, 1 g / mL EDC solution and 1 g / mL NHS solution were added to the composite solution, and the solution was poured into a mold after rapid stirring for 30 seconds. The mold was placed in a water bath and heated at 80°C for 3 minutes. After that, the solution solidified into a hydrogel 1, namely, a conductive protein marine polysaccharide hydrogel dressing 1 (BPPR-1 hydrogel).
[0053] Example 2
[0054] 1. Preparation of Ru-TA Nanorods 2
[0055] (1) F127 was dissolved in a 13.04% ethanol solution (volume ratio of ethanol to water 1:6.67) and stirred until completely dissolved. Then, 28% ammonia water was added to the mixed solvent, the pH was adjusted to 9-12, the volume ratio of ammonia water to the mixed solvent was 1:180, and stirred for 1 hour. Tannic acid was then added to the solution, stirred for 24 hours, and RuCl was added. 3 ·3H 2 O, stirred for 24 h, 0.0037 g F127, 0.0037 g tannic acid and 0.00185 g RuCl were added per ml of ethanol solution. 3 ·3H 2 O.
[0056] (2) The solution was transferred to a hydrothermal reactor, which was placed in an oven and heated to 100°C for 24 hours. After the reactor was cooled to room temperature naturally, the solution in the reactor was transferred to a centrifuge tube and centrifuged at 8000 rpm for 10 minutes.
[0057] (3) removing the supernatant from the centrifuge tube, adding deionized water for vortex washing, and then centrifuging again to remove the supernatant. Repeating the above washing and centrifugation steps for 3 times, freeze-drying the final precipitate to obtain a powder, which is Ru-TA nanorods 2.
[0058] 2. Preparation of Conductive Protein Marine Polysaccharide Hydrogel Dressing 2
[0059] (1) A 0.33 wt % PEDOT:PSS aqueous solution, a 1 g / mL EDC solution and a 1 g / mL NHS solution were prepared, and the volume ratio of the PEDOT:PSS aqueous solution, the EDC solution and the NHS solution was 1:0.02:0.02.
[0060] (2) BSA, fucoidan and Ru-TA nanorods 2 were added to a 0.33 wt % PEDOT:PSS aqueous solution and stirred for 30 min. 0.17 g BSA, 0.017 g fucoidan and 0.0017 g Ru-TA nanorods 2 were added to each milliliter of PEDOT:PSS aqueous solution.
[0061] (3) Then, 1 g / mL EDC solution and 1 g / mL NHS solution were added to the composite solution. After rapid stirring for 30 seconds, the solution was poured into a mold. The mold was placed in a water bath and heated at 80°C for 3 minutes. After that, the solution solidified into hydrogel 2, namely, conductive protein marine polysaccharide hydrogel dressing 2 (BPPR-2 hydrogel).
[0062] Example 3
[0063] 1. Preparation of Ru-TA Nanorods 3
[0064] (1) F127 was dissolved in a 13.04% ethanol solution (volume ratio of ethanol to water 1:6.67) and stirred until completely dissolved. Then, 28% ammonia water was added to the mixed solvent, the pH was adjusted to 9-12, the volume ratio of ammonia water to the mixed solvent was 1:108, and stirred for 1 hour. Tannic acid was then added to the solution, stirred for 24 hours, and RuCl was added. 3 ·3H 2 O, stirred for 24 h, 0.0037 g F127, 0.0056 g tannic acid and 0.0026 g RuCl were added per ml of ethanol solution. 3 ·3H 2 O.
[0065] (2) The solution was transferred to a hydrothermal reactor, which was placed in an oven and heated to 100°C for 24 hours. After the reactor was cooled to room temperature naturally, the solution in the reactor was transferred to a centrifuge tube and centrifuged at 8000 rpm for 10 minutes.
[0066] (3) removing the supernatant from the centrifuge tube, adding deionized water for vortex washing, and then centrifuging again to remove the supernatant. Repeating the above washing and centrifugation steps for 3 times, freeze-drying the final precipitate to obtain a powder, which is Ru-TA nanorods 3.
[0067] 2. Preparation of Conductive Protein Marine Polysaccharide Hydrogel Dressing 3
[0068] (1) A 0.43 wt % PEDOT:PSS aqueous solution, a 1 g / mL EDC solution and a 1 g / mL NHS solution were prepared, and the volume ratio of the PEDOT:PSS aqueous solution, the EDC solution and the NHS solution was 1:0.015:0.015.
[0069] (2) BSA, fucoidan and Ru-TA nanorods 3 were added to a 0.43 wt % PEDOT:PSS aqueous solution and stirred for 30 min. 0.17 g BSA, 0.034 g fucoidan and 0.0034 g Ru-TA nanorods 3 were added to each milliliter of the PEDOT:PSS aqueous solution.
[0070] (3) Then, 1 g / mL EDC solution and 1 g / mL NHS solution were added to the composite solution, and the solution was poured into a mold after rapid stirring for 30 seconds. The mold was placed in a water bath and heated at 80°C for 3 minutes. After that, the solution solidified into hydrogel 3, namely, conductive protein marine polysaccharide hydrogel dressing 3 (BPPR-3 hydrogel).
[0071] Comparative Example 1
[0072] Preparation of hydrogel dressing D1:
[0073] (1) Prepare 1 g / mL EDC solution and 1 g / mL NHS solution. The volume ratio of deionized water, EDC solution and NHS solution is 1:0.015:0.015.
[0074] (2) Add BSA and chitosan to deionized water, add 0.17 g BSA and 0.0085 g chitosan per ml of deionized water, and stir for 30 min.
[0075] (3) Then, 1 g / mL EDC solution and 1 g / mL NHS solution were added to the composite solution, and the solution was poured into the mold after rapid stirring for 30 s. The mold was placed in a water bath and heated at 80 °C for 3 min, and the solution solidified into hydrogel D1, i.e., BP hydrogel.
[0076] Comparative Example 2
[0077] Preparation of hydrogel dressing D2:
[0078] (1) A 0.22 wt % PEDOT:PSS aqueous solution, a 1 g / mL EDC solution and a 1 g / mL NHS solution were prepared, and the volume ratio of the PEDOT:PSS aqueous solution, the EDC solution and the NHS solution was 1:0.015:0.015.
[0079] (2) Add BSA and chitosan to a 0.22 wt % PEDOT:PSS aqueous solution. Add 0.17 g BSA and 0.0085 g chitosan to each milliliter of PEDOT:PSS aqueous solution and stir for 30 min.
[0080] (3) Then, 1 g / mL EDC solution and 1 g / mL NHS solution were added to the composite solution, and the solution was poured into the mold after rapid stirring for 30 s. The mold was placed in a water bath and heated at 80 °C for 3 min, and the solution solidified into hydrogel D2, i.e., BPP hydrogel.
[0081] Example 4
[0082] Performance test of BPPR-1, 2, 3 hydrogels:
[0083] 1. Optical Microscope Image and TEM Image Analysis
[0084] The optical image and TEM image of Ru-TA nanorods 2 were taken using an inverted fluorescence microscope and a transmission electron microscope, respectively.
[0085] like Figure 1 and Figure 2 As shown, the Ru-TA nanorod 2 is a rod-like structure with a length of 2-8 μm, indicating that the present invention successfully prepared a metal-polyphenol network with a regular morphology by hydrothermal synthesis.
[0086] 2. FTIR images of BPPR-2 hydrogel
[0087] The FTIR results of BPPR-2 hydrogel are shown in Figure 3 As shown. 3318cm -1 The characteristic peak at 2962cm is the stretching vibration of -OH. -1 The characteristic peak at 1658cm is the CH stretching vibration. -1 The characteristic peak is C=O stretching vibration. 1537cm -1 The characteristic peak at 1235cm is the NH bending vibration. -1 The characteristic peak at 832cm is the CN stretching vibration. -1 The characteristic peak at is the COS stretching vibration of the sulfate group.
[0088] 3. Conductivity test of BPPR-1, 2, 3 hydrogels, BP hydrogels, and BPP hydrogels
[0089] The specific test method is as follows:
[0090] (1) First, the hydrogel is cut into discs using a circular mold. The hydrogel discs are soaked in deionized water until swelling equilibrium is reached.
[0091] (2) Take out the hydrogel disc that has swelled in deionized water and absorb the water on the surface with absorbent paper.
[0092] (3) Use a vernier caliper to measure the thickness and diameter of the hydrogel disc, and place the hydrogel in the center of the sample stage of the conductivity meter. Adjust the probe height until it touches the surface of the hydrogel. Enter the size parameters of the hydrogel in the software, adjust the instrument current to an appropriate range, and measure the conductivity of the hydrogel.
[0093] The results are as follows Figure 4As shown. The conductivity of BP hydrogel without PEDOT:PSS is poor. The conductivity of BPP hydrogel and BPPR-1, 2, and 3 hydrogels containing PEDOT:PSS is significantly higher than that of BP hydrogel. As the content of PEDOT:PSS in the hydrogel gradually increases, the conductivity of BPPR hydrogel gradually increases. This shows that PEDOT:PSS, as a water-soluble highly conductive polymer, can effectively improve the electrical activity of the hydrogel. The conductivity of the prepared BPPR-3 hydrogel reached 1.58×10 -3 S / cm. Hydrogels with high electrical activity as a medium can more efficiently conduct externally applied electrical stimulation, thereby accelerating the healing speed of the wound site.
[0094] 4. BPPR-3 hydrogel removes H 2 O 2 test
[0095] H 2 O 2 is one of the most common ROS. 2 O 2 The scavenging effect can reflect its antioxidant capacity.
[0096] The specific test method is as follows:
[0097] (1) First, Ti(SO 4 ) 2 Dissolved in diluted H 2 SO 4 Configuration Ti(SO 4 ) 2 Solution.
[0098] (2) Add 1 mM H 2 O 2 and 0.2 g of hydrogel in a centrifuge tube, and place the tube at 37 °C for 2 h. After 2 h, take the supernatant in the centrifuge tube and mix it with Ti(SO 4 ) 2 The solution was mixed.
[0099] (3) After 30 minutes, take 1 mL of the mixed solution into a cuvette and measure the scanning curve of the solution in the cuvette using a UV-visible spectrophotometer. At the same time, measure the absorbance value at 405 nm and calculate the hydrogel's H 2 O 2 clearance rate.
[0100] The test results are as follows Figure 5 and Figure 6 As shown, BP hydrogel and BPP hydrogel have 2 O 2The scavenging effect of BP hydrogel and BPP hydrogel was weak, which may be due to the ROS scavenging activity of marine polysaccharides contained in the hydrogel. However, the ROS scavenging effect of BP hydrogel and BPP hydrogel was not ideal from the scanning curve and scavenging effect. 2 O 2 The clearance rate is only about 11%. Therefore, it is necessary to improve the antioxidant properties of the hydrogel by adding materials with strong ROS scavenging activity. The results show that the BPPR-3 hydrogel with the addition of Ru-TA has a much stronger H than the BP and BPP hydrogels. 2 O 2 The clearance capacity, H 2 O 2 The removal rate was 84.9%. This shows that Ru-TA nanorods have excellent H 2 O 2 Scavenging activity, loading in hydrogel can significantly improve the antioxidant properties of hydrogel.
[0101] 5. Cell Proliferation without and with Electrical Stimulation
[0102] The results of cell proliferation were tested under no electrical stimulation and electrical stimulation conditions. The specific test steps are as follows:
[0103] (1) The cells were inoculated in a culture dish and cultured for 2-3 times before use in subsequent experiments. The hydrogel material was sterilized with alcohol and then used for later use.
[0104] (2) Treat the cells in the culture dish with trypsin to prepare a cell suspension, then inoculate it into a 24-well plate. Place the 24-well plate in a 37°C incubator until the cells are completely attached to the bottom of the well plate.
[0105] (3) The prepared sterilized hydrogel was then co-cultured with the cells, and the culture medium was replaced every 2 days during the culture process. The electrical stimulation group also needed to use a laboratory-made metal scaffold to perform external electrical stimulation on the cells. The metal scaffold was sterilized with alcohol and dried before use, and was placed on the surface of the hydrogel after adding the hydrogel material to conduct the electric field through the hydrogel.
[0106] (4) The electrical stimulation group received electrical stimulation for 30 minutes every day. The non-electrical stimulation group did not use metal stents for electrical stimulation and cultured cells normally. After culturing the cells for 3 days, the hydrogel was removed and CCK-8 working solution was added to measure the relative number of cells. The cell survival rate of each group was calculated by measuring the absorbance value at 450nm. The cell survival rate of the control group was set to 100%.
[0107] The results are as follows Figure 7As shown, the number of cells in the control group increased under electrical stimulation, indicating the promoting effect of electrical stimulation on cell proliferation. Due to its poor electrical conductivity, the BP hydrogel did not show obvious cell proliferation effect under electrical stimulation. However, the number of cells in the BPP hydrogel and BPPR-3 hydrogel with higher electrical conductivity increased significantly under electrical stimulation, and the cell survival rates were 203.6% and 201.4%, respectively. The number of cells was twice that of the control group. It is proved that hydrogel materials with excellent electrical conductivity combined with electrical stimulation can greatly promote cell proliferation.
[0108] 6. Fluorescence images of cells stained with DCFH-DA and DAPI
[0109] DCFH-DA is used to detect the level of cellular ROS, and DAPI is used to stain the cell nucleus. The higher the level of ROS in the cell, the stronger the fluorescence of DCFH-DA. The specific experimental steps are as follows:
[0110] (1) First, cells were seeded in a 24-well plate. The seeding procedure was similar to that of the cell proliferation experiment.
[0111] (2) An equal amount of ROS solution was added to all wells, and the sterilized hydrogel discs were co-cultured with the corresponding cells.
[0112] (3) Place the well plate in a 37°C incubator for 24 hours, then take it out and add DCFH-DA fluorescent probe and DAPI to stain the cells. After staining, use an inverted fluorescence microscope to take fluorescent images of DCFH-DA and DAPI staining of the cells in the 24-well plate.
[0113] The results are as follows Figure 8 As shown. In the control group, the DCFH-DA fluorescence of cells was very strong due to the presence of ROS. However, due to the weak ability of BP hydrogel and BPP hydrogel to scavenge ROS, the DCFH-DA fluorescence of cells was not significantly weakened compared with the control group. However, there was only weak DCFH-DA fluorescence in cells treated with BPPR-3 hydrogel, indicating that ROS in this group were effectively scavenged. This result is also consistent with the previous results on scavenging H 2 O 2 The results of the tests were similar.
[0114] 7. Wound healing assay
[0115] (1) The prepared BPPR-3 hydrogel was sterilized and set aside for later use, and the experimental instruments were disinfected. First, the rats were anesthetized and the hair on their backs was removed. The skin on the backs of the rats was disinfected with alcohol.
[0116] (2) A skin wound model was then constructed on the back of the rats, and the wound was treated with sterilized BPPR-3 hydrogel. After the experiment began, the wound was photographed every few days and new hydrogel materials were replaced. The electrical stimulation group received electrical stimulation for 30 minutes every day.
[0117] The results are as follows Fig. 9 and Fig.10 . Seven days after wound modeling, the control group still had more than half of the wound area. The wounds treated with BPPR-3 hydrogel had healed 93.2%. Under external electrical stimulation, the effect of BPPR-3 hydrogel treatment was further improved, and the wound healed 96.3%. This result shows that BPPR-3 hydrogel itself has excellent therapeutic effect on wounds, and the combination of this hydrogel and external electrical stimulation can further accelerate the healing speed of wounds.
[0118] Although the above embodiments have been described in detail, they are only a part of the embodiments of the present invention, not all of them. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all belong to the protection scope of the present invention.
Claims
1. A method for preparing a conductive protein marine polysaccharide hydrogel dressing, characterized in that: The following steps are involved: (1) preparing a poly(3,4-ethylenedioxythiophene)-poly(styrene sulfonic acid) aqueous solution, a 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride solution, and an N-hydroxysuccinimide solution; (2) adding bovine serum albumin, marine polysaccharide and Ru-TA nanorods to a poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) aqueous solution and stirring to obtain a composite solution; (3) Add 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride solution and N-hydroxysuccinimide solution to the composite solution, stir rapidly to obtain a mixed solution, pour the mixed solution into a mold, place the mold in a water bath and heat at high temperature, and the solution solidifies into a hydrogel to obtain a conductive protein marine polysaccharide hydrogel dressing.
2. The method for preparing the hydrogel dressing according to claim 1, characterized in that: In the step 1), the concentration of the poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) aqueous solution is 0.22wt% to 0.65wt%; the concentration of the 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride solution is 1g / mL; and the concentration of the N-hydroxysuccinimide solution is 1g / mL.
3. The method for preparing the hydrogel dressing according to claim 2, characterized in that: In the step 1), the volume ratio of the poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) aqueous solution, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride solution and N-hydroxysuccinimide solution is 1:0.01-0.02:0.01-0.
02.
4. The method for preparing the hydrogel dressing according to claim 2 or 3, characterized in that: In the step 1), the volume ratio of the poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) aqueous solution, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride solution and N-hydroxysuccinimide solution is 1:0.015:0.
015.
5. The method for preparing the hydrogel dressing according to claim 1, characterized in that: In the step 2), the marine polysaccharide is chitosan or fucoidan; the mass ratio of bovine serum albumin, marine polysaccharide and Ru-TA nanorods is 1:0.05-0.5:0.005-0.03; 0.17 g of bovine serum albumin is added to each milliliter of poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) aqueous solution.
6. The method for preparing the hydrogel dressing according to claim 1 or 5, characterized in that: In the step 2), the concentration of the poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) aqueous solution is 0.43wt%; 0.17g of bovine serum albumin, 0.034g of fucoidan and 0.0034g of Ru-TA nanorods are added to each milliliter of the poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) aqueous solution.
7. The method for preparing the hydrogel dressing according to claim 1, characterized in that: The preparation method of the Ru-TA nanorods is as follows: (1) Poloxamer is dissolved in an ethanol solution and stirred until completely dissolved, then aqueous ammonia is added to the solution to adjust the pH to 9 to 12, then tannic acid is added to the solution and stirred, and ruthenium trichloride is added and stirred; (2) transferring the solution to a hydrothermal reactor, placing the hydrothermal reactor in an oven for heating, reacting, waiting for the reactor to cool naturally to room temperature, and centrifuging; (3) removing the supernatant from the centrifuge tube, adding deionized water for vortex washing, and then centrifuging again to remove the supernatant. Repeating the above washing and centrifugation steps for 3 times, the final precipitate product is freeze-dried to obtain Ru-TA nanorod powder.
8. The method for preparing Ru-TA nanorods according to claim 7, characterized in that: In the step 1), the mass ratio of poloxamer, tannic acid and ruthenium trichloride is 1:0.5-2:0.1-1; the volume fraction of the ethanol solution is 8%-25%; and 0.0037g of poloxamer is added to each milliliter of ethanol solution.
9. The method for preparing Ru-TA nanorods according to claim 6, characterized in that: In the step 1), the volume fraction of the ethanol solution is 13.04%; 0.0037 g of poloxamer, 0.0056 g of tannic acid and 0.0026 g of ruthenium trichloride are added to each milliliter of the ethanol solution.
10. Use of the conductive protein marine polysaccharide hydrogel dressing prepared by the preparation method of claim 1 in preparing products for improving cell proliferation and wound healing.
Citation Information
Cited By
Photocuring conductive hybrid nano hydrogel based on MPN-PEDOT: PSS as well as preparation method and application of photocuring conductive hybrid nano hydrogel
CN121154926A
A photocured conductive hybrid nanohydrogel based on MPN-PEDOT:PSS and a preparation method and application thereof
CN121154926B