Preparation process of paper-like film and packaging bag
By introducing antibacterial fillers and epoxy resins into the polypropylene imitation paper film, the problem of the lack of antibacterial properties of the polypropylene imitation paper film is solved, which significantly improves the antibacterial properties and durability, and extends the product's shelf life , reducing replacement frequency and cost.
Patent Information
- Application Number
- CN202410952523.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
The polypropylene imitation paper film lacks antibacterial properties, resulting in bacterial growth, the product has a short shelf life and needs to be replaced frequently, which increases the cost.
Using a paper-imitation film preparation process, grafting SEBS, calcium stearate, antibacterial filler, antioxidant 1010 and epoxy resin by mixing polypropylene, low-density polyethylene, dibenzylidene sorbitol, maleic anhydride, SEBS, calcium stearate, antibacterial filler, antioxidant 1010 and epoxy resin. Perform melting, hot pressing molding and corona treatment to prepare a imitation paper film with antibacterial properties, and by preparing antibacterial fillers, zinc ions, aluminum-titanium coupling agents and nano-silver colloids are used to form a mesh crosslinking structure. Enhance antibacterial effect.
It significantly improves the antibacterial properties and durability of imitation paper films, can effectively sterilize and extend the shelf life of the product, and reduces the replacement frequency and cost.
Smart Images

Figure BDA0004947616050000061 
Figure BDA0004947616050000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of packaging bag preparation, and in particular relates to a preparation process of an imitation paper film and a packaging bag. Background Art
[0002] Biaxially oriented polypropylene paper-like film is a film made of polypropylene (PP) material through a biaxial stretching process. This film is similar to paper in appearance, touch and performance, so it is widely used in packaging, labeling, printing and other fields. Since there is no functional group in the molecular structure of polypropylene that can provide antibacterial activity, and it is difficult to introduce antibacterial chemical components inside or on the surface of the material, it has always been a technical problem to achieve antibacterial function in polypropylene materials. Polypropylene packaging bags with poor antibacterial effects may become a breeding ground for microorganisms, leading to bacterial growth. Due to the lack of antibacterial properties, polypropylene packaging bags cannot extend the shelf life of the product and need to be replaced more frequently, thereby increasing costs. Summary of the invention
[0003] The object of the present invention is to provide a preparation process of a paper-like film and a packaging bag, so as to improve the antibacterial property of the polypropylene paper-like film.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A preparation process of a paper-like film, comprising the following steps:
[0006] Polypropylene (purchased from Shanghai Maclean Biochemical Technology Co., Ltd.), low-density polyethylene (purchased from Shanghai Maclean Biochemical Technology Co., Ltd.), dibenzylidene sorbitol (purchased from Xishi Chemical Technology (Shanghai) Co., Ltd.), maleic anhydride grafted SEBS (purchased from Tai'an Jiayue Biochemical Co., Ltd.), calcium stearate, antibacterial filler, antioxidant 1010 (purchased from Guangzhou Dayin New Materials Co., Ltd.), epoxy resin (purchased from Jinan Chuangshi Chemical Co., Ltd.), trimellitic anhydride are mixed, melted at 160-180°C, filtered, vented 10-15 times, each venting time is 8-12s, hot-pressed at 10-20MPa, stretched, and corona treated to obtain the paper-like film.
[0007] As a preferred technical solution of the present invention, the mass ratio of polypropylene, low-density polyethylene, dibenzylidene sorbitol, maleic anhydride grafted SEBS, calcium stearate, antibacterial filler, antioxidant 1010, epoxy resin, and trimellitic anhydride is 70-80:10-15:1-2:2-3:1-2:1-2:0.6-0.8:6-8:0.3-0.5.
[0008] As a preferred technical solution of the present invention, the preparation method of the antibacterial filler comprises the following steps:
[0009] S1. Mix zinc acetate, 2-mercaptobenzimidazole, methanol and deionized water, stir for 2-3 hours, let stand for 20-30 hours, centrifuge, wash and dry the solid phase to obtain material A;
[0010] S2, taking the material A, aluminum-titanium composite coupling agent (purchased from Wuhan Kamik Technology Co., Ltd.), and n-hexane, mixing them, stirring at 40-50° C. for 8-10 hours, to obtain material B;
[0011] S3, taking the material B, nanosilver colloid (purchased from Nanjing Xianfeng Nanomaterial Technology Co., Ltd.), and anhydrous ethanol, mixing, ultrasonically dispersing for 20-30 minutes, and drying at 40° C. for 4-6 hours to obtain the antibacterial filler.
[0012] As a preferred technical solution of the present invention, in step S1, the dosage ratio of zinc acetate, 2-mercaptobenzimidazole, methanol and deionized water is 0.3-0.32 g: 0.16-0.17 g: 150 mL: 50 mL.
[0013] As a preferred technical solution of the present invention, in step S2, the mass ratio of the material A, the aluminum-titanium composite coupling agent, and n-hexane is 3-4:0.2-0.3:100.
[0014] As a preferred technical solution of the present invention, in step S3, the dosage ratio of the material B, the nanosilver colloid and the anhydrous ethanol is 2-3g:200mL:100mL.
[0015] As a preferred technical solution of the present invention, in step S3, the concentration of the nanosilver colloid is 1 g / L.
[0016] The paper-like film is prepared by using the above-mentioned paper-like film preparation process.
[0017] The packaging bag is made by using the above-mentioned imitation paper film, and the preparation method of the packaging bag comprises the following steps:
[0018] The packaging bag is obtained by flattening and fixing the kraft paper, applying adhesive on the surface of the kraft paper, covering the imitation paper film, pressing, drying, cutting, shaping and bagging.
[0019] As a preferred technical solution of the present invention, the length of the kraft paper is 100 cm, the width is 80 cm, and the thickness is 0.0012 cm; the length of the imitation paper film is 100 cm, the width is 80 cm, and the thickness is 0.3 cm; the amount of the adhesive uniformly applied to the surface of the kraft paper is 2 g / m 2 ; The adhesive is white latex (purchased from Zhongshan Youxing Enterprise Adhesive Products Co., Ltd.).
[0020] Beneficial effects of the present invention:
[0021] The invention discloses a preparation process of a paper-like film and a packaging bag, which can release zinc ions to generate electrostatic action with bacterial cell walls to kill bacteria by preparing antibacterial fillers; introduces an aluminum-titanium coupling agent with antibacterial effect to modify the surface of the filler to form a network cross-linked structure to hold nanosilver, thereby further achieving antibacterial efficacy; and simultaneously introduces imidazole groups to polymerize with epoxy resin to increase the density of the paper-like film and improve the antibacterial durability. DETAILED DESCRIPTION
[0022] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.
[0023] The method for preparing a packaging bag using an imitation paper film comprises the following steps:
[0024] Take kraft paper, lay it flat, fix it, apply adhesive on the surface of the kraft paper, cover it with the imitation paper film, press it, dry it, cut it, shape it, and make it into a bag to obtain the packaging bag; the kraft paper has a length of 100 cm, a width of 80 cm, and a thickness of 0.0012 cm; the imitation paper film has a length of 100 cm, a width of 80 cm, and a thickness of 0.3 cm; the adhesive is evenly applied to the surface of the kraft paper in an amount of 2 g / m 2 ; The adhesive is white latex.
[0025] Example 1
[0026] The preparation process of the paper-like film comprises the following steps:
[0027] Polypropylene, low-density polyethylene, dibenzylidene sorbitol, maleic anhydride grafted SEBS, calcium stearate, antibacterial filler, antioxidant 1010, epoxy resin, and trimellitic anhydride are mixed, melted at 160°C, filtered, vented 10 times, each venting takes 8 seconds, hot-pressed at 10 MPa, stretched, and corona treated to obtain the paper-like film; the mass ratio of the polypropylene, low-density polyethylene, dibenzylidene sorbitol, maleic anhydride grafted SEBS, calcium stearate, antibacterial filler, antioxidant 1010, epoxy resin, and trimellitic anhydride is 70:10:1:2:1:1:0.6:6:0.3;
[0028] The preparation method of the antibacterial filler comprises the following steps:
[0029] S1. Mix zinc acetate, 2-mercaptobenzimidazole, methanol and deionized water, stir for 2 hours, let stand for 20 hours, centrifuge, wash the solid phase, and dry to obtain material A; the dosage ratio of zinc acetate, 2-mercaptobenzimidazole, methanol and deionized water is 0.3g:0.16g:150mL:50mL;
[0030] S2, taking the material A, the aluminum-titanium composite coupling agent, and n-hexane, mixing them, stirring at 40° C. for 8 hours, to obtain material B; the mass ratio of the material A, the aluminum-titanium composite coupling agent, and n-hexane is 3:0.2:100;
[0031] S3, taking the material B, nanosilver colloid, and anhydrous ethanol, mixing, ultrasonically dispersing for 20 minutes, and drying at 40° C. for 4 hours to obtain the antibacterial filler; the amount ratio of the material B, nanosilver colloid, and anhydrous ethanol is 2g:200mL:100mL; the concentration of the nanosilver colloid is 1g / L.
[0032] Example 2
[0033] The preparation process of the paper-like film comprises the following steps:
[0034] Polypropylene, low-density polyethylene, dibenzylidene sorbitol, maleic anhydride grafted SEBS, calcium stearate, antibacterial filler, antioxidant 1010, epoxy resin, and trimellitic anhydride are mixed, melted at 170°C, filtered, vented 12 times, each venting takes 10 seconds, hot-pressed at 15MPa, stretched, and corona treated to obtain the paper-like film; the mass ratio of the polypropylene, low-density polyethylene, dibenzylidene sorbitol, maleic anhydride grafted SEBS, calcium stearate, antibacterial filler, antioxidant 1010, epoxy resin, and trimellitic anhydride is 75:13:1.5:2.5:1.5:1.5:0.7:7:0.4;
[0035] The preparation method of the antibacterial filler comprises the following steps:
[0036] S1. Mix zinc acetate, 2-mercaptobenzimidazole, methanol and deionized water, stir for 2.5 hours, let stand for 25 hours, centrifuge, wash the solid phase, and dry to obtain material A; the dosage ratio of zinc acetate, 2-mercaptobenzimidazole, methanol and deionized water is 0.31 g: 0.165 g: 150 mL: 50 mL;
[0037] S2, taking the material A, the aluminum-titanium composite coupling agent, and n-hexane, mixing them, stirring at 45° C. for 9 hours, to obtain material B; the mass ratio of the material A, the aluminum-titanium composite coupling agent, and n-hexane is 3.5:0.25:100;
[0038] S3, taking the material B, nanosilver colloid, and anhydrous ethanol, mixing, ultrasonically dispersing for 25 minutes, and drying at 40° C. for 5 hours to obtain the antibacterial filler; the amount ratio of the material B, nanosilver colloid, and anhydrous ethanol is 2.5g:200mL:100mL; the concentration of the nanosilver colloid is 1g / L.
[0039] Example 3
[0040] The preparation process of the paper-like film comprises the following steps:
[0041] Polypropylene, low-density polyethylene, dibenzylidene sorbitol, maleic anhydride grafted SEBS, calcium stearate, antibacterial filler, antioxidant 1010, epoxy resin, and trimellitic anhydride are mixed, melted at 180°C, filtered, vented 15 times, each venting takes 12 seconds, hot-pressed at 20 MPa, stretched, and corona treated to obtain the paper-like film; the mass ratio of the polypropylene, low-density polyethylene, dibenzylidene sorbitol, maleic anhydride grafted SEBS, calcium stearate, antibacterial filler, antioxidant 1010, epoxy resin, and trimellitic anhydride is 80:15:2:3:2:2:0.8:8:0.5;
[0042] The preparation method of the antibacterial filler comprises the following steps:
[0043] S1. Mix zinc acetate, 2-mercaptobenzimidazole, methanol and deionized water, stir for 3 hours, let stand for 30 hours, centrifuge, wash the solid phase, and dry to obtain material A; the dosage ratio of zinc acetate, 2-mercaptobenzimidazole, methanol and deionized water is 0.32g:0.17g:150mL:50mL;
[0044] S2, taking the material A, the aluminum-titanium composite coupling agent, and n-hexane, mixing them, stirring at 50° C. for 10 hours, to obtain material B; the mass ratio of the material A, the aluminum-titanium composite coupling agent, and n-hexane is 4:0.3:100;
[0045] S3, taking the material B, nanosilver colloid, and anhydrous ethanol, mixing, ultrasonically dispersing for 30 minutes, and drying at 40° C. for 6 hours to obtain the antibacterial filler; the amount ratio of the material B, nanosilver colloid, and anhydrous ethanol is 3g:200mL:100mL; the concentration of the nanosilver colloid is 1g / L.
[0046] Comparative Example 1
[0047] The difference from Example 1 is that the preparation method of the antibacterial filler comprises the following steps:
[0048] S1. Mix zinc acetate, 2-mercaptobenzimidazole, methanol and deionized water, stir for 2 hours, let stand for 20 hours, centrifuge, wash the solid phase, and dry to obtain material A; the dosage ratio of zinc acetate, 2-mercaptobenzimidazole, methanol and deionized water is 0.3g:0.16g:150mL:50mL;
[0049] S2. Mix the material A, nanosilver colloid and anhydrous ethanol, disperse them by ultrasonication for 20 minutes, and dry them at 40°C for 4 hours to obtain the antibacterial filler; the dosage ratio of the material A, nanosilver colloid and anhydrous ethanol is 2g:200mL:100mL; the concentration of the nanosilver colloid is 1g / L.
[0050] Comparative Example 2
[0051] The difference from Comparative Example 1 is that the preparation method of the antibacterial filler comprises the following steps:
[0052] Nanosilver colloid and anhydrous ethanol are mixed, ultrasonically dispersed for 20 minutes, and dried at 40° C. for 4 hours to obtain the antibacterial filler; the dosage ratio of the nanosilver colloid and anhydrous ethanol is 200 mL:100 mL; the concentration of the nanosilver colloid is 1 g / L.
[0053] Comparative Example 3
[0054] The difference from Example 1 is that no epoxy resin is added during the preparation of the paper-like film.
[0055] Performance Testing
[0056] The paper-like films prepared in Example 1 to Example 3 and Comparative Example 1 to Comparative Example 3 were tested for antibacterial performance according to standard GB / T 31402-2015; the antibacterial rate was tested according to standard T / CPP IA 17-2022; and the antibacterial persistence was tested according to standard JC / T939-2004. The results are shown in Table 1 below.
[0057] Table 1
[0058]
[0059]
[0060] As shown in Table 1, the paper-like films prepared in Examples 1-3 of the present application have excellent antibacterial durability and antibacterial performance. In Comparative Example 1, no titanium-containing coupling agent was introduced, resulting in a decrease in antibacterial performance; in Comparative Example 2, only a silver-containing antibacterial agent was used, resulting in a significant decrease in antibacterial effect; in Comparative Example 3, no epoxy resin was added, resulting in a decrease in antibacterial durability.
[0061] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A process for preparing a paper-like film, characterized in that: The preparation process of the paper-like film comprises the following steps: Polypropylene, low-density polyethylene, dibenzylidene sorbitol, maleic anhydride grafted SEBS, calcium stearate, antibacterial filler, antioxidant 1010, epoxy resin and trimellitic anhydride are mixed, melted at 160-180° C., filtered, vented 10-15 times, each venting time is 8-12 seconds, hot-pressed at 10-20 MPa, stretched, and corona treated to obtain the paper-like film.
2. The process for preparing a paper-like film according to claim 1, characterized in that: The mass ratio of the polypropylene, low-density polyethylene, dibenzylidene sorbitol, maleic anhydride grafted SEBS, calcium stearate, antibacterial filler, antioxidant 1010, epoxy resin and trimellitic anhydride is 70-80:10-15:1-2:2-3:1-2:1-2:0.6-0.8:6-8:0.3-0.
5.
3. The process for preparing a paper-like film according to claim 1, characterized in that: The preparation method of the antibacterial filler comprises the following steps: S1. Mix zinc acetate, 2-mercaptobenzimidazole, methanol and deionized water, stir for 2-3 hours, let stand for 20-30 hours, centrifuge, wash and dry the solid phase to obtain material A; S2, taking the material A, the aluminum-titanium composite coupling agent and n-hexane, mixing them, stirring at 40-50° C. for 8-10 hours, to obtain material B; S3, taking the material B, nanosilver colloid, and anhydrous ethanol, mixing them, ultrasonically dispersing them for 20-30 minutes, and drying them at 40° C. for 4-6 hours to obtain the antibacterial filler.
4. The process for preparing a paper-like film according to claim 3, characterized in that: In step S1, the dosage ratio of zinc acetate, 2-mercaptobenzimidazole, methanol and deionized water is 0.3-0.32 g: 0.16-0.17 g: 150 mL: 50 mL.
5. The process for preparing a paper-like film according to claim 3, characterized in that: In step S2, the mass ratio of material A, aluminum-titanium composite coupling agent and n-hexane is 3-4:0.2-0.3:
100.
6. The process for preparing a paper-like film according to claim 3, characterized in that: In step S3, the dosage ratio of the material B, the nanosilver colloid and the anhydrous ethanol is 2-3 g: 200 mL: 100 mL.
7. The process for preparing a paper-like film according to claim 3, characterized in that: In step S3, the concentration of the nanosilver colloid is 1 g / L.
8. A paper-like film obtained by the process for preparing a paper-like film according to any one of claims 1 to 7.
9. A packaging bag made of the imitation paper film as claimed in claim 8, characterized in that: The method for preparing the packaging bag comprises the following steps: The packaging bag is obtained by flattening and fixing the kraft paper, applying adhesive on the surface of the kraft paper, covering the imitation paper film, pressing, drying, cutting, shaping and bagging.
10. The packaging bag according to claim 9, characterized in that: The length of the kraft paper is 100 cm, the width is 80 cm, and the thickness is 0.0012 cm; the length of the imitation paper film is 100 cm, the width is 80 cm, and the thickness is 0.3 cm; the amount of the adhesive uniformly applied on the surface of the kraft paper is 2 g / m 2 ; The adhesive is white latex.