High-temperature-resistant thermal insulation coating, preparation method and application of high-temperature-resistant thermal insulation coating in petrochemical pipelines
By using high-temperature insulation coatings combined with silicone modified acrylic aqueous dispersion and modified hollow glass microbeads in petrochemical pipelines, the problems of insufficient corrosion resistance and complex construction are solved, and high-efficiency thermal insulation and chemical stability are achieved simplifies the construction process and reduces costs.
Patent Information
- Application Number
- CN202411165139.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-23
AI Technical Summary
Traditional porous thermal insulation materials have insufficient corrosion resistance in petrochemical pipelines, resulting in corrosion factors being easily attached and stored in pores, reducing thermal insulation efficiency, increasing safety hazards, and complex construction and high cost.
High-temperature insulation coatings combined with silicone modified acrylic aqueous dispersion and modified hollow glass microbeads are used to improve the high-temperature resistance and chemical stability of the coatings through modification treatment, and nanoreflective powder is added to enhance the reflective thermal insulation effect. .
It improves the high temperature resistance, aging resistance and chemical stability of the coating, reduces heat absorption, enhances adhesion and impact resistance, simplifies the construction process, reduces costs, and improves the thermal insulation effect of petrochemical pipelines.
Smart Images

Figure BDA0005007641370000121
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of coatings, and in particular to a high temperature resistant heat-insulating coating, a preparation method and application thereof in petrochemical pipelines. Background Art
[0002] In the petrochemical industry, the energy lost due to heat dissipation in pipelines accounts for about one-third of the total energy consumption each year, and the corrosion of petrochemical pipelines also brings many safety hazards to its production and operation. Therefore, anti-corrosion and thermal insulation are very important for the petrochemical industry.
[0003] At present, domestic refining and chemical companies usually use traditional porous rock wool, aluminum silicate felt, etc. to insulate equipment and pipelines. The thickness of the insulation layer can generally reach 100-200mm, and the construction process is complicated and costly. In addition, the thick insulation layer will also cover up the damage of equipment and pipelines, making it difficult for petrochemical companies to avoid conventional production risks and safety hazards. At the same time, the insulation layer of special-shaped parts such as elbows, tees, and valves has a complex structure, many interfaces, and great construction difficulty. These parts are often exposed and are the weak link in the insulation of equipment and pipelines. In particular, traditional porous insulation materials often do not have corrosion resistance, and corrosion factors can easily adhere to and be stored in their pores, becoming a medium for heat conduction, which not only greatly reduces the insulation efficiency of equipment and pipelines, but also shortens the service life of the entire insulation system.
[0004] CN1935912A discloses a nano-ceramic high-temperature resistant thermal insulation coating and a preparation method thereof, which improves the high-temperature resistance and thermal insulation performance of the coating by adding ceramic microspheres. The nano-ceramic microspheres added to the nano-ceramic high-temperature resistant thermal insulation coating prepared by the method may have poor interfacial compatibility with the film-forming material. CN115873456A discloses a water-based high-temperature resistant coating and a preparation method thereof, which improves the high-temperature resistance of the coating by adding mixed water-based resin and functional modified powder. The coating prepared by the method mainly uses reflective insulation and radiation insulation, and cannot achieve the effect of thermal insulation. Summary of the invention
[0005] In view of the above-mentioned defects of the prior art, the object of the present invention is to provide a high temperature resistant thermal insulation coating having the advantages of high temperature resistance, good thermal insulation performance and strong chemical stability.
[0006] To achieve the above object, the present invention provides a high temperature resistant thermal insulation coating and a preparation method thereof.
[0007] The detailed technical scheme of the present invention is as follows:
[0008] A high temperature resistant thermal insulation coating, comprising the following raw materials:
[0009] By mass, the ingredients include 100-140 parts of silicone-modified acrylic aqueous dispersion, 10-30 parts of modified hollow glass microspheres, 10-30 parts of curing agent, 5-10 parts of nano-reflective powder, 2-4 parts of additives, and 20-40 parts of water.
[0010] The organosilicon-modified acrylic acid aqueous dispersion is prepared by the following method:
[0011] 100-125 parts of a solvent are heated to 110-140° C. under nitrogen protection, and a mixture of 15-20 parts of glycidyl acrylate, 15-20 parts of methyl methacrylate, 15-20 parts of benzyl acrylate, 15-20 parts of acrylic acid and 1-2 parts of an initiator is added dropwise to the solvent within 1-3 hours. After the dropwise addition is completed, 5-15 parts of dimethylphenylvinylsilane are added thereto within 5-15 minutes, and 0.1-1 parts of the initiator are additionally added, and the mixture is reacted at 110-140° C. and 600-800 rpm for 2-4 hours; the temperature is lowered to 60-80° C., 120-180 parts of water are added, and the mixture is stirred at 600-800 rpm for 5-10 minutes, and diethanolamine is added to adjust the pH to 6-8 to obtain an organic silicon-modified acrylic acid aqueous dispersion.
[0012] The initiator is azobisisobutyronitrile.
[0013] As a further illustration of the present invention: the organosilicon-modified acrylic aqueous dispersion uses glycidyl acrylate, methyl methacrylate, benzyl acrylate, and acrylic acid as mixed monomers to synthesize a polymer that can improve chemical properties, wherein the benzyl acrylate molecular structure contains a benzene ring that can increase strength and improve chemical properties and water resistance when preparing the polymer; methyl methacrylate can improve the flexibility and impact resistance of the polymer when preparing the polymer; glycidyl acrylate can improve the adhesion of the polymer when preparing the polymer; the carboxyl group contained in the acrylic acid molecular structure can be further used for cross-linking or reaction with other monomers, and the mixed monomer can improve physical and chemical properties and cross-linking strength.
[0014] The modified hollow glass microspheres are prepared by the following method:
[0015] By mass, 10-30 parts of hollow glass microspheres are dried at 100-140° C. for 2-4 hours, added into 100-150 parts of ethanol, stirred at 50-70° C. and 600-800 rpm for 5-10 minutes, 1-3 parts of coupling agent are added, reacted for 20-40 minutes, and then filtered. The obtained hollow glass microspheres are dried at 100-140° C. for 2-4 hours, filtered through a 200-mesh filter, and sealed to obtain modified hollow glass microspheres.
[0016] The coupling agent is an aluminate coupling agent.
[0017] As a further explanation of the present invention: Hollow glass microspheres are a kind of hollow material with the characteristics of low density, high strength, low thermal conductivity, etc., and a large amount of still air is wrapped inside, so the thermal conductivity of hollow glass microspheres is usually only 0.05-0.1W / (m·K). However, as an inorganic material, hollow glass microspheres have poor interfacial compatibility with organic emulsions, so there are often a lot of gaps between the two, resulting in an increase in the water absorption rate of the coating dry film. The surface modification of the coupling agent can improve the interfacial compatibility between the hollow glass microspheres and the organic emulsion.
[0018] The curing agent is at least one of isocyanate and aziridine.
[0019] The nano reflective powder is at least one of nano titanium dioxide, nano zinc oxide and nano silicon dioxide.
[0020] The auxiliary agent is at least one of a defoamer, a dispersant and an antioxidant.
[0021] The present invention provides a method for preparing a high temperature resistant thermal insulation coating, and the preparation method is as follows:
[0022] Step 1: Evenly mix 100-140 parts of silicone-modified acrylic acid aqueous dispersion and 10-30 parts of modified hollow glass microspheres for later use;
[0023] Step 2: Mix 10-30 parts of curing agent, 2-4 parts of auxiliary agent, 5-10 parts of nano reflective powder and 20-40 parts of water and stir evenly for later use;
[0024] Step 3: Stir and mix the mixture obtained in step 1 and step 2 to obtain a high temperature resistant thermal insulation coating;
[0025] The above parts are parts by mass.
[0026] Beneficial effects of the present invention:
[0027] Compared with the existing technology, the coating uses silicone-modified acrylic water-based dispersion and modified hollow glass microspheres. These ingredients work together to improve the coating's high temperature resistance, aging resistance and chemical stability. DETAILED DESCRIPTION
[0028] A high temperature resistant thermal insulation coating, comprising the following raw materials:
[0029] Calculated by mass, it includes 100-140 parts of silicone-modified acrylic aqueous dispersion, 10-30 parts of modified hollow glass microspheres, 10-30 parts of curing agent, 5-10 parts of nano-reflective powder, 2-4 parts of auxiliary agent and 20-40 parts of water.
[0030] The organosilicon-modified acrylic acid aqueous dispersion is prepared by the following method:
[0031] 100-125 parts of a solvent are heated to 110-140° C. under nitrogen protection, and a mixture of 15-20 parts of glycidyl acrylate, 15-20 parts of methyl methacrylate, 15-20 parts of benzyl acrylate, 15-20 parts of acrylic acid and 1-2 parts of an initiator are added dropwise to the solvent within 1-3 hours. After the addition is completed, 5-15 parts of dimethylphenylvinylsilane are added thereto within 5-15 minutes, and 0.1-1 parts of the initiator are additionally added, and the mixture is reacted at 110-140° C. and 600-800 rpm for 2-4 hours; the temperature is lowered to 60-80° C., 120-180 parts of water are added, and the mixture is stirred at 600-800 rpm for 5-10 minutes, and diethanolamine is added to adjust the pH to 6-8 to obtain an organic silicon-modified acrylic acid aqueous dispersion.
[0032] The organosilicon-modified acrylic aqueous dispersion uses glycidyl acrylate, methyl methacrylate, benzyl acrylate, and acrylic acid as mixed monomers to synthesize polymers to improve chemical properties, wherein the benzyl acrylate molecular structure contains a benzene ring, which can improve strength and improve chemical properties and water resistance when preparing polymers; methyl methacrylate can improve the flexibility and impact resistance of polymers prepared by preparing polymers; glycidyl acrylate can improve its adhesion; the carboxyl group contained in the acrylic acid molecular structure can be further used for cross-linking or reacting with other monomers, and the mixed monomer can improve physical and chemical properties and cross-linking strength. The acrylic resin prepared by the organosilicon-modified mixed monomer exhibits good high temperature resistance and aging resistance, while retaining good chemical resistance, flexibility, impact resistance, waterproof performance and adhesion.
[0033] The modified hollow glass microspheres are prepared by the following method:
[0034] By mass, 10-30 parts of hollow glass microspheres are dried at 100-140° C. for 2-4 hours, added into 100-150 parts of ethanol, stirred at 50-70° C. and 600-800 rpm for 5-10 minutes, 1-3 parts of coupling agent are added, reacted for 20-40 minutes, and then filtered. The obtained hollow glass microspheres are dried at 100-140° C. for 2-4 hours, filtered through a 200-mesh filter, and sealed to obtain modified hollow glass microspheres.
[0035] Hollow glass microspheres are hollow materials with low density, high strength, and low thermal conductivity. They contain a large amount of still air, so the thermal conductivity of hollow glass microspheres is usually only 0.05-0.1W / (m·K). However, as an inorganic material, hollow glass microspheres have poor interfacial compatibility with organic emulsions, so there are often a lot of gaps between the two, which leads to an increase in the water absorption of the coating dry film. The surface modification of the hollow glass microspheres with coupling agents can improve their interfacial compatibility with organic emulsions. The silanol groups on the surface of the hollow glass microspheres undergo dehydration condensation with the hydroxyl groups formed after the hydrolysis of the coupling agent, and a very small monolayer of the organic end of the coupling agent is grafted on the surface of the hollow glass microspheres by forming ─Si─O─Si─. At the same time, because the matrix is still hollow glass microspheres (SiO2), it retains good chemical properties and improves its interfacial compatibility with organic emulsions.
[0036] The curing agent is at least one of isocyanate and aziridine.
[0037] The nano reflective powder is at least one of nano titanium dioxide, nano zinc oxide and nano silicon dioxide.
[0038] The above-mentioned nanomaterials all have high reflectivity, can reflect visible light and infrared light in sunlight, can scatter incident light, reduce light penetration, and thus reduce heat absorption.
[0039] The auxiliary agent is at least one of a defoamer, a dispersant and an antioxidant.
[0040] The present invention provides a method for preparing a high temperature resistant thermal insulation coating, and the preparation method is as follows:
[0041] Step 1: Evenly mix 100-140 parts of silicone-modified acrylic acid aqueous dispersion and 10-30 parts of modified hollow glass microspheres for later use;
[0042] Step 2: Mix 10-30 parts of curing agent, 2-4 parts of auxiliary agent, 5-10 parts of nano reflective powder and 20-40 parts of water and stir evenly for later use;
[0043] Step 3: Stir and mix the mixture obtained in step 1 and step 2 to obtain a high temperature resistant thermal insulation coating.
[0044] The sources and parameters of some chemical substances in the examples are as follows:
[0045] Glycidyl acrylate, CAS No.: 106-90-1;
[0046] Polydimethylsiloxane, CAS No.: 63148-62-9, viscosity 0.65 cSt (25°C), from Shanghai Aladdin Biochemical Technology Co., Ltd.;
[0047] BYK-028 and BYK-301, from BYK Chemicals;
[0048] Dimethylchlorosilane, CAS number: 1066-35-9;
[0049] Dimethylphenylvinylsilane, CAS number: 1125-26-4;
[0050] Nano titanium dioxide, particle size: 5-10nm;
[0051] Nano zinc oxide, particle size 20nm;
[0052] Hollow glass microspheres, model: HL38, true density (g / cm 3 ): 0.38, D50 (μm): 40, D90 (μm): 65, compressive strength: 5500psi, floating rate: ≥95%, moisture content: ≤3%, from Zhengzhou Shenglait Hollow Microsphere New Materials Co., Ltd.
[0053] Isopropyl distearoyl aluminate, CAS: 5919-73-3;
[0054] Isopropyl tri(dioctyl pyrophosphate) titanate, CAS: 67691-13-8;
[0055] Isocyanate, CAS number: 75-13-8.
[0056] Example 1
[0057] A method for preparing a high temperature resistant thermal insulation coating comprises the following steps:
[0058] Step 1: Mix 100g of silicone-modified acrylic acid aqueous dispersion and 10g of modified hollow glass microspheres for later use;
[0059] Step 2: Mix 20g of curing agent, 2g of auxiliary agent, 8g of nano reflective powder and 40g of water and stir evenly for later use;
[0060] Step 3: Stir and mix the mixture obtained in step 1 and step 2 to obtain a high temperature resistant thermal insulation coating.
[0061] The organosilicon-modified acrylic acid aqueous dispersion in step 1 is prepared by the following method:
[0062] Under nitrogen protection, 75g of a mixed solvent of propylene glycol methyl ether and 25g of butanol was heated to 125°C, and a mixture of 15g of glycidyl acrylate, 15g of methyl methacrylate, 15g of benzyl acrylate, 15g of acrylic acid and 1g of azobisisobutyronitrile was added dropwise to the solvent within 2 hours. After the dropwise addition was completed, 5g of dimethylphenylvinylsilane was added thereto within 10 minutes, and 0.5g of azobisisobutyronitrile was added, and the mixture was reacted at 125°C and 800rpm for 3 hours; the temperature was lowered to 70°C, 150g of water was added, and the mixture was stirred at 800rpm for 5 minutes, and diethanolamine was added to adjust the pH to 8 to obtain an organic silicon-modified acrylic aqueous dispersion.
[0063] The modified hollow glass microspheres in step 1 are prepared by the following method:
[0064] After drying 10 g of hollow glass microspheres at 120° C. for 2 h, add them to 100 g of ethanol, stir at 60° C. and 800 rpm for 5 min, add 2 g of isopropyl distearoyloxyaluminate, react for 30 min, and then filter. After drying the obtained hollow glass microspheres at 120° C. for 2 h, filter them through a 200-mesh filter, and seal them to obtain modified hollow glass microspheres.
[0065] The curing agent is isocyanate.
[0066] The auxiliary agents are 0.5 g of defoamer BYK-028 and 1.5 g of dispersant BYK-301.
[0067] The nano reflective powder is a mixture of nano titanium dioxide and nano zinc oxide in a mass ratio of 1:1.
[0068] Example 2
[0069] A method for preparing a high temperature resistant thermal insulation coating comprises the following steps:
[0070] Step 1: Mix 100g of silicone-modified acrylic acid aqueous dispersion and 10g of modified hollow glass microspheres for later use;
[0071] Step 2: Mix 20g of curing agent, 2g of auxiliary agent, 8g of nano reflective powder and 40g of water and stir evenly for later use;
[0072] Step 3: Stir and mix the mixture obtained in step 1 and step 2 to obtain a high temperature resistant thermal insulation coating.
[0073] The organosilicon-modified acrylic acid aqueous dispersion in step 1 is prepared by the following method:
[0074] Under nitrogen protection, 75g of a mixed solvent of propylene glycol methyl ether and 25g of butanol was heated to 125°C, and a mixture of 15g of glycidyl acrylate, 15g of methyl methacrylate, 15g of benzyl acrylate, 15g of acrylic acid and 1g of azobisisobutyronitrile was added dropwise to the solvent within 2 hours. After the addition was completed, 5g of polydimethylsiloxane was added thereto within 10 minutes, and 0.5g of azobisisobutyronitrile was added, and the mixture was reacted at 125°C and 800rpm for 3 hours; the temperature was lowered to 70°C, 150g of water was added, and the mixture was stirred at 800rpm for 5 minutes, and diethanolamine was added to adjust the pH to 8 to obtain an organic silicon-modified acrylic aqueous dispersion.
[0075] The modified hollow glass microspheres in step 1 are prepared by the following method:
[0076] After drying 10 g of hollow glass microspheres at 120° C. for 2 h, add them to 100 g of ethanol, stir at 60° C. and 800 rpm for 5 min, add 2 g of isopropyl distearoyloxyaluminate, react for 30 min, and then filter. After drying the obtained hollow glass microspheres at 120° C. for 2 h, filter them through a 200-mesh filter, and seal them to obtain modified hollow glass microspheres.
[0077] The curing agent is isocyanate.
[0078] The auxiliary agents are 0.5 g of defoamer BYK-028 and 1.5 g of dispersant BYK-301.
[0079] The nano reflective powder is a mixture of nano titanium dioxide and nano zinc oxide in a mass ratio of 1:1.
[0080] Example 3
[0081] A method for preparing a high temperature resistant thermal insulation coating comprises the following steps:
[0082] Step 1: Mix 100g of silicone-modified acrylic acid aqueous dispersion and 10g of modified hollow glass microspheres for later use;
[0083] Step 2: Mix 20g of curing agent, 2g of auxiliary agent, 8g of nano reflective powder and 40g of water and stir evenly for later use;
[0084] Step 3: Stir and mix the mixture obtained in step 1 and step 2 to obtain a high temperature resistant thermal insulation coating.
[0085] The organosilicon-modified acrylic acid aqueous dispersion in step 1 is prepared by the following method:
[0086] Under nitrogen protection, 75g of a mixed solvent of propylene glycol methyl ether and 25g of butanol was heated to 125°C, and a mixture of 15g of glycidyl acrylate, 15g of methyl methacrylate, 15g of benzyl acrylate, 15g of acrylic acid and 1g of azobisisobutyronitrile was added dropwise to the solvent within 2 hours. After the addition was completed, 5g of dimethylchlorosilane was added within 10 minutes, and 0.5g of azobisisobutyronitrile was added, and the mixture was reacted at 125°C and 800rpm for 3 hours; the temperature was lowered to 70°C, 150g of water was added, and the mixture was stirred at 800rpm for 5 minutes, and diethanolamine was added to adjust the pH to 8 to obtain an organic silicon-modified acrylic acid aqueous dispersion.
[0087] The modified hollow glass microspheres in step 1 are prepared by the following method:
[0088] After drying 10 g of hollow glass microspheres at 120° C. for 2 h, add them to 100 g of ethanol, stir at 60° C. and 800 rpm for 5 min, add 2 g of isopropyl distearoyloxyaluminate, react for 30 min, and then filter. After drying the obtained hollow glass microspheres at 120° C. for 2 h, filter them through a 200-mesh filter, and seal them to obtain modified hollow glass microspheres.
[0089] The curing agent is isocyanate.
[0090] The auxiliary agents are 0.5 g of defoamer BYK-028 and 1.5 g of dispersant BYK-301.
[0091] The nano reflective powder is a mixture of nano titanium dioxide and nano zinc oxide in a mass ratio of 1:1.
[0092] Comparative Example 1
[0093] A method for preparing a high temperature resistant thermal insulation coating comprises the following steps:
[0094] Step 1: Mix 100g of acrylic acid aqueous dispersion and 10g of modified hollow glass microspheres evenly for later use;
[0095] Step 2: Mix 20g of curing agent, 2g of auxiliary agent, 8g of nano reflective powder and 40g of water and stir evenly for later use;
[0096] Step 3: Stir and mix the mixture obtained in step 1 and step 2 to obtain a high temperature resistant thermal insulation coating.
[0097] The acrylic acid aqueous dispersion in step 1 is prepared by the following method:
[0098] Under nitrogen protection, 75 g of a mixed solvent of propylene glycol methyl ether and 25 g of butanol was heated to 125° C., and a mixture of 15 g of glycidyl acrylate, 15 g of methyl methacrylate, 15 g of benzyl acrylate, 15 g of acrylic acid and 1 g of azobisisobutyronitrile was added dropwise into the solvent within 2 h, and the mixture was reacted at 125° C. and 800 rpm for 3 h; the temperature was lowered to 70° C., 150 g of water was added, and the mixture was stirred at 800 rpm for 5 min, and diethanolamine was added to adjust the pH to 8 to obtain an aqueous acrylic acid dispersion.
[0099] The modified hollow glass microspheres in step 1 are prepared by the following method:
[0100] After drying 10 g of hollow glass microspheres at 120° C. for 2 h, add them to 100 g of ethanol, stir at 60° C. and 800 rpm for 5 min, add 2 g of isopropyl distearoyloxyaluminate, react for 30 min, and then filter. After drying the obtained hollow glass microspheres at 120° C. for 2 h, filter them through a 200-mesh filter, and seal them to obtain modified hollow glass microspheres.
[0101] The curing agent is isocyanate.
[0102] The auxiliary agents are 0.5 g of defoamer BYK-028 and 1.5 g of dispersant BYK-301.
[0103] The nano reflective powder is a mixture of nano titanium dioxide and nano zinc oxide in a mass ratio of 1:1.
[0104] Comparative Example 2
[0105] A method for preparing a high temperature resistant thermal insulation coating comprises the following steps:
[0106] Step 1: Mix 100g of silicone-modified acrylic acid aqueous dispersion and 10g of hollow glass microspheres evenly for later use;
[0107] Step 2: Mix 20g of curing agent, 2g of auxiliary agent, 8g of nano reflective powder and 40g of water and stir evenly for later use;
[0108] Step 3: Stir and mix the mixture obtained in step 1 and step 2 to obtain a high temperature resistant thermal insulation coating.
[0109] The organosilicon-modified acrylic acid aqueous dispersion in step 1 is prepared by the following method:
[0110] Under nitrogen protection, 75g of a mixed solvent of propylene glycol methyl ether and 25g of butanol was heated to 125°C, and a mixture of 15g of glycidyl acrylate, 15g of methyl methacrylate, 15g of benzyl acrylate, 15g of acrylic acid and 1g of azobisisobutyronitrile was added dropwise to the solvent within 2 hours. After the dropwise addition was completed, 5g of dimethylphenylvinylsilane was added thereto within 10 minutes, and 0.5g of azobisisobutyronitrile was added, and the mixture was reacted at 125°C and 800rpm for 3 hours; the temperature was lowered to 70°C, 150g of water was added, and the mixture was stirred at 800rpm for 5 minutes, and diethanolamine was added to adjust the pH to 8 to obtain an organic silicon-modified acrylic aqueous dispersion.
[0111] The curing agent is isocyanate.
[0112] The auxiliary agents are 0.5 g of defoamer BYK-028 and 1.5 g of dispersant BYK-301.
[0113] The nano reflective powder is a mixture of nano titanium dioxide and nano zinc oxide in a mass ratio of 1:1.
[0114] Comparative Example 3
[0115] A method for preparing a high temperature resistant thermal insulation coating comprises the following steps:
[0116] Step 1: Mix 100g of silicone-modified acrylic acid aqueous dispersion and 10g of modified hollow glass microspheres for later use;
[0117] Step 2: Mix 20g of curing agent, 2g of auxiliary agent, 8g of nano reflective powder and 40g of water and stir evenly for later use;
[0118] Step 3: Stir and mix the mixture obtained in step 1 and step 2 to obtain a high temperature resistant thermal insulation coating.
[0119] The organosilicon-modified acrylic acid aqueous dispersion in step 1 is prepared by the following method:
[0120] Under nitrogen protection, 75g of a mixed solvent of propylene glycol methyl ether and 25g of butanol was heated to 125°C, and a mixture of 15g of glycidyl acrylate, 15g of methyl methacrylate, 15g of benzyl acrylate, 15g of acrylic acid and 1g of azobisisobutyronitrile was added dropwise to the solvent within 2 hours. After the dropwise addition was completed, 5g of dimethylphenylvinylsilane was added thereto within 10 minutes, and 0.5g of azobisisobutyronitrile was added, and the mixture was reacted at 125°C and 800rpm for 3 hours; the temperature was lowered to 70°C, 150g of water was added, and the mixture was stirred at 800rpm for 5 minutes, and diethanolamine was added to adjust the pH to 8 to obtain an organic silicon-modified acrylic aqueous dispersion.
[0121] The modified hollow glass microspheres in step 1 are prepared by the following method:
[0122] After drying 10 g of hollow glass microspheres at 120° C. for 2 h, add them to 100 g of ethanol, stir at 60° C. and 800 rpm for 5 min, add 2 g of isopropyl tri(dioctyl pyrophosphate) titanate, react for 30 min, and then filter. After drying the obtained hollow glass microspheres at 120° C. for 2 h, filter them through a 200-mesh filter, and seal them to obtain modified hollow glass microspheres.
[0123] The curing agent is isocyanate.
[0124] The auxiliary agents are 0.5 g of defoamer BYK-028 and 1.5 g of dispersant BYK-301.
[0125] The nano reflective powder is a mixture of nano titanium dioxide and nano zinc oxide in a mass ratio of 1:1.
[0126] Test Example 1
[0127] The following performance tests were conducted on the high temperature resistant thermal insulation coatings with different formulations, and the results are listed in Table 1:
[0128] Test the adhesion of the coating according to GB / T 5210-2006 "Determination of adhesion of paints and varnishes by pull-off method";
[0129] GB / T 23987-2009 “Artificial weathering of paint and varnish coatings - Exposure to fluorescent UV light and water”;
[0130] High temperature resistance test: Apply the freshly prepared coating on a clean steel plate with a coating thickness of 300μm. After the surface is dry, dry it in a 60℃ constant temperature drying oven for 120min, take it out and cool it naturally in the room for 24h, and then bake the coating sample at 100℃ and 200℃ for 10h.
[0131] Table 1
[0132]
[0133] By comparing Examples 1-3, it can be found that the high temperature resistant thermal insulation coating of Example 1 has the best adhesion. The possible reason is that the acrylic aqueous dispersion modified with dimethylphenylvinylsilane is added. The acrylic aqueous dispersion modified with silicone can improve the adhesion between the coating and the substrate. The addition of dimethylphenylvinylsilane to the coating can further increase the crosslinking density of the coating, enhance the chemical bonding force between the coating and the substrate, and thus improve the adhesion.
[0134] By comparing Examples 1-3 with Comparative Example 3, it can be found that the high temperature resistance and aging resistance of the high temperature resistant thermal insulation coatings of Examples 1-3 are significantly better than those of Comparative Example 3. The reason is that Examples 1-3 add hollow glass beads modified with aluminate coupling agents, while Comparative Example 3 adds hollow glass beads modified with titanate coupling agents. While the inorganic end of the aluminate coupling agent reacts with the hydroxyl groups on the surface of the hollow glass microspheres to generate ─Si─O─Si─, some aluminum ions will form metal coordination bonds with the oxygen atoms in the hydroxyl groups on the surface of the hollow glass microspheres, so that the aluminate coupling agent can be grafted on the surface of the hollow glass microspheres very well. The metal central atom in the aluminate coupling agent, aluminum, is a trivalent metal with two organic reaction groups. Compared with the titanate coupling agent, it has better compatibility with the polymer emulsion and can form a denser coating structure, thereby improving its high temperature resistance and aging resistance.
Claims
1. A high temperature resistant thermal insulation coating, characterized in that: Calculated by mass, it includes 100-140 parts of silicone-modified acrylic aqueous dispersion, 10-30 parts of modified hollow glass microspheres, 10-30 parts of curing agent, 5-10 parts of nano-reflective powder, 2-4 parts of auxiliary agent and 20-40 parts of water.
2. The high temperature resistant heat insulation coating according to claim 1, characterized in that: The organosilicon-modified acrylic acid aqueous dispersion is prepared by the following method: 100-125 parts of a solvent are heated to 110-140° C. under nitrogen protection, and a mixture of 15-20 parts of glycidyl acrylate, 15-20 parts of methyl methacrylate, 15-20 parts of benzyl acrylate, 15-20 parts of acrylic acid and 1-2 parts of an initiator are added dropwise to the solvent within 1-3 hours. After the addition is completed, 5-15 parts of dimethylphenylvinylsilane are added thereto within 5-15 minutes, and 0.1-1 parts of the initiator are additionally added, and the mixture is reacted at 110-140° C. and 600-800 rpm for 2-4 hours; the temperature is lowered to 60-80° C., 120-180 parts of water are added, and the mixture is stirred at 600-800 rpm for 5-10 minutes, and diethanolamine is added to adjust the pH to 6-8 to obtain an organic silicon-modified acrylic acid aqueous dispersion.
3. The high temperature resistant heat insulation coating according to claim 2, characterized in that: The initiator is azobisisobutyronitrile.
4. The high temperature resistant heat insulation coating according to claim 1, characterized in that: The modified hollow glass microspheres are prepared by the following method: By mass, 10-30 parts of hollow glass microspheres are dried at 100-140° C. for 2-4 hours, added into 100-150 parts of ethanol, stirred at 50-70° C. and 600-800 rpm for 5-10 minutes, 1-3 parts of coupling agent are added, reacted for 20-40 minutes, and then filtered. The obtained hollow glass microspheres are dried at 100-140° C. for 2-4 hours, filtered through a 200-mesh filter, and sealed to obtain modified hollow glass microspheres.
5. The high temperature resistant heat insulation coating according to claim 4, characterized in that: The coupling agent is an aluminate coupling agent.
6. The high temperature resistant heat insulation coating according to claim 1, characterized in that: The curing agent is at least one of isocyanate and aziridine.
7. The high temperature resistant heat insulation coating according to claim 1, characterized in that: The nano reflective powder is at least one of nano titanium dioxide, nano zinc oxide and nano silicon dioxide.
8. The high temperature resistant heat insulation coating according to claim 1, characterized in that: The auxiliary agent is at least one of a defoamer, a dispersant and an antioxidant.
9. The method for preparing the high temperature resistant thermal insulation coating according to any one of claims 1 to 8, characterized in that: The synthesis steps include: Step 1: Evenly mix 100-140 parts of silicone-modified acrylic acid aqueous dispersion and 10-30 parts of modified hollow glass microspheres for later use; Step 2: Mix 10-30 parts of curing agent, 2-4 parts of auxiliary agent, 5-10 parts of nano reflective powder and 20-40 parts of water and stir evenly for later use; Step 3: Stir and mix the mixture obtained in step 1 and step 2 to obtain a high temperature resistant thermal insulation coating; The above parts are parts by mass.
10. Use of the high temperature resistant thermal insulation coating according to any one of claims 1 to 8 in petrochemical pipelines.
Citation Information
Patent Citations
Method for preparing anticorrosive paint for directly-buried thermal power pipeline insulating layer
CN102775863A
Thin-layer heat-preserving insulation coating material
CN104530859A
Elastic thermal insulation coating for outer walls and preparation method of coating
CN112521842A
Ultra-early-stage water-resistant silicon modified waterborne polyurethane coating and preparation method thereof
CN116023852A
Water-based functional coating, color-coated sheet and preparation processes of water-based functional coating and color-coated sheet
CN117820923A