Resin composition for back coating of thermal transfer ribbon, back coating and preparation method of back coating

The combination of high TG value linear non-crystalline polyester resin and gas-phase nanosilicon dioxide modified with silicone modified acrylate and silane coupling agent is solved. The lack of heat resistance and slippage has achieved efficient printing performance and matte visual effect.

CN118909522AActive Publication Date: 2024-11-08HANGZHOU TODAYTEC DIGITAL
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411148605.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-08
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

The existing thermal transfer ribbon back coating has insufficient heat resistance and slippage under high temperature conditions, resulting in poor printhead contamination and matte effect, and the commonly used matting agents have settled and agglomerated during application. Disadvantages such as uneven physical properties of the membrane.

Method used

The resin composition is prepared by a specific grinding process using a linear non-crystalline polyester resin combined with silicone modified acrylate and a gas-phase nanosilica modified with silane coupling agent to form an excellent printing performance. and matte visual effects back coat.

Benefits of technology

It realizes continuous printing without material residue under high temperature conditions, meets high breakdown energy level, high weather resistance, high film formation and low noise performance, while improving the stability of the coating and matte visual effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005002937880000031
    Figure BDA0005002937880000031
  • Figure BDA0005002937880000041
    Figure BDA0005002937880000041
  • Figure BDA0005002937880000061
    Figure BDA0005002937880000061
Patent Text Reader

Abstract

The invention provides a resin composition for back coating of a heat transfer printing ribbon, a back coating layer and a preparation method of the back coating layer, and relates to the technical field of heat transfer printing. The resin composition for back coating of the heat transfer printing ribbon comprises the following components in parts by weight: 2-15 parts of linear amorphous polyester resin with a high TG value, 1-2 parts of organic silicon modified acrylate, 0.5-2 parts of a delustering agent and 30-100 parts of a solvent, wherein the high-TG-value linear amorphous polyester resin comprises first modified polyester resin and second modified polyester resin in a mass ratio of (2-8): (0-3); the first modified polyester resin has a B-type structure; the second modified polyester resin has an L-shaped structure; and the TG value of the high-TG-value linear amorphous polyester resin is 50 DEG C or more. The resin composition disclosed by the invention is excellent in printing continuity, and meets high breakdown energy level, high compatibility, high heat resistance, high smoothness and low noise performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermal transfer printing, and in particular to a resin composition for back coating of a thermal transfer ribbon, a back coating layer and a preparation method thereof. Background Art

[0002] Thermal transfer ribbon is composed of a ribbon base (such as PET film), a thermal transfer coating and a back coating coated on its surface. During the printing process, the ink layer is melted and transferred to the medium through the heating element of the thermal print head. The thermal transfer back coating is an important coating. Since the ribbon needs to withstand the high temperature generated instantly by the thermal print head during the thermal transfer process, a back coating needs to be coated on one side of the substrate. The back coating needs to have not only high heat resistance, but also good smoothness to ensure the smoothness of the transfer process. More importantly, the back coating needs to have excellent adhesion to the substrate to ensure that the glue does not fall off during the long-term transfer process to avoid contamination of the print head.

[0003] Matt coatings have developed rapidly in recent years, and the optical properties of their coatings have become increasingly important. Matt coatings can usually be made by adding a matting agent. The matte back coating of thermal transfer ribbons is different from the general thermal transfer back coating. Matt coatings achieve the matte purpose by adding a matting agent, and the thermal transfer matte back coating needs to adapt to the heat resistance and smoothness requirements of thermal transfer printing. However, the addition of a matting agent will lead to poor friction resistance and poor permeability.

[0004] At present, the matting agents commonly used in this field include inorganic or organic matting agents such as silicon dioxide, talcum powder, polyurethane, and polyacrylate particles. Organic matting agents have good effects on wetting ability and coating uniformity, but in the process of thermal transfer printing, the high temperature of the print head will cause the properties of the organic matting agent to change, resulting in difficulty in film removal or shedding and accumulation around the print head, which will eventually make the printing unclear or even damage the print head. General inorganic matting agents, such as silica particle matting agents, have the disadvantages of sedimentation and agglomeration, low coating properties, and uneven surface optical effects during the application process. Therefore, at present, gas-phase nano-silica is mostly used instead of ordinary silica. Although it can absorb more resin, thereby appropriately reducing sedimentation and agglomeration, and increasing the coating properties and optical uniformity; however, too much adhesive will still increase the viscosity of the coating, causing the powder particles to be suspended in the coating and not easy to settle, and will also cause the coating to be not lubricated enough, which will then cause the thermal transfer carbon belt to be difficult to remove the film, easy to break through, and unable to adapt to the use function of the thermal transfer ribbon.

[0005] In addition, resin is needed to bond and fix the back coating of thermal transfer ribbon with matte agent. The back coating of thermal transfer ribbon with matte function first meets the requirements of back coating with matte effect, so all raw materials such as resin, additives, matte agent, etc. that increase the matte effect need to adapt to the basic requirements of back coating, such as solvent, compatibility, heat resistance, smoothness, printing noise requirements, etc.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] The object of the present invention is to provide a resin composition for back coating of thermal transfer ribbon, a back coating layer and a preparation method thereof. The resin composition of the present invention adopts a linear non-crystalline polyester resin with a specific structure and a silicone-modified acrylate, has excellent printing conditions, can ensure that there is no material residue near the print head after continuous printing, and simultaneously meets multiple properties such as high breakdown energy level, high compatibility, high heat resistance, high smoothness and low noise performance, and can reflect an excellent matte visual effect.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] In a first aspect, the present invention provides a resin composition for a back coating of a thermal transfer ribbon, wherein the resin composition for a back coating of a thermal transfer ribbon comprises the following components in parts by weight:

[0010]

[0011]

[0012] Among them, the high TG value linear non-crystalline polyester resin includes a first modified polyester resin and a second modified polyester resin in a mass ratio of (2 to 8): (0 to 3); the first modified polyester resin has a B-type structure; the second modified polyester resin has an L-type structure; and the TG value of the high TG value linear non-crystalline polyester resin is above 50°C.

[0013] Furthermore, the molecular weight of the first modified polyester resin is 8000-12000.

[0014] Furthermore, the TG value of the first modified polyester resin is 55-65°C.

[0015] Furthermore, the hydroxyl value of the first modified polyester resin is 6 to 8 KOHmg / g.

[0016] Furthermore, the acid value of the first modified polyester resin is 6 to 8 KOHmg / g.

[0017] Furthermore, the first modified polyester resin is modified polyester GK255 resin.

[0018] Furthermore, the molecular weight of the second modified polyester resin is 1000-5000.

[0019] Furthermore, the TG value of the second modified polyester resin is 50-55°C.

[0020] Furthermore, the hydroxyl value of the second modified polyester resin is 45 to 55 KOHmg / g.

[0021] Furthermore, the second modified polyester resin is modified polyester 220 resin.

[0022] Furthermore, the matting agent is gas-phase nano-silica modified by a silane coupling agent.

[0023] Furthermore, the silane coupling agent is KH570.

[0024] Furthermore, the particle size of the gas-phase nano-silicon dioxide is 30 to 50 nm.

[0025] Furthermore, the specific surface area of ​​the fumed nano-silicon dioxide is 160 to 200 m 2 / g.

[0026] Furthermore, the solvent includes any one of xylene, butanone or toluene, or a combination of at least two thereof, preferably a mixed solution of butanone and toluene, a mixed solution of butanone and xylene, or a mixed solution of butanone, toluene and xylene.

[0027] Furthermore, the mass ratio of xylene, butanone and toluene is (0-4):(1-2):(0-4).

[0028] Furthermore, the resin composition for thermal transfer ribbon back coating comprises the following components in parts by weight:

[0029]

[0030] In a second aspect, the present invention provides a method for preparing the resin composition for back coating of a thermal transfer ribbon as described in the first aspect, the preparation method comprising the following steps:

[0031] The various raw materials in the resin composition for the back coating of the thermal transfer ribbon are mixed and then ground to obtain the resin composition for the back coating of the thermal transfer ribbon.

[0032] Furthermore, the method for preparing the resin composition for thermal transfer ribbon back coating specifically comprises the following steps:

[0033] Dissolving the high TG value linear non-crystalline polyester resin in a solvent to obtain a resin solution, dispersing a matting agent in the resin solution, and performing a first grinding to obtain a dispersion;

[0034] The dispersion and the organosilicon-modified acrylate are mixed and ground for a second time to obtain the resin composition for back coating of the thermal transfer ribbon.

[0035] Furthermore, the first grinding and / or the second grinding is performed using a sand mill.

[0036] Furthermore, the particle size of the dispersion obtained by the first grinding is less than 2 μm.

[0037] Furthermore, the particle size of the resin composition obtained by the second grinding is less than 0.6 μm.

[0038] In a third aspect, the present invention provides a thermal transfer back coating layer, wherein the thermal transfer back coating layer is formed by curing the resin composition for thermal transfer ribbon back coating as described in the first aspect.

[0039] In a fourth aspect, the present invention provides a method for preparing the thermal transfer back coating according to the third aspect, the preparation method comprising the following steps:

[0040] The resin composition for thermal transfer ribbon back coating as described in the first aspect is coated on the surface of the substrate and cured by baking to obtain the thermal transfer back coating.

[0041] Furthermore, the coating amount of the resin composition for back coating of the thermal transfer ribbon is 0.2 to 0.4 g / m 2 .

[0042] Furthermore, the baking temperature is 50-60°C.

[0043] Furthermore, the baking time is 5 to 9 seconds.

[0044] Compared with the prior art, the present invention has the following beneficial effects:

[0045] (1) The resin composition of the present invention adopts a linear non-crystalline polyester resin with a high TG value of a specific structure and a silicone-modified acrylate to further improve the printing performance, ensure that there is no material residue near the print head after continuous printing, and at the same time meet multiple performances such as high breakdown energy level, high weather resistance, high heat resistance, high film-forming property, high smoothness and low noise performance.

[0046] (2) The resin composition of the present invention uses a specific matting agent silane coupling agent modified gas-phase nano-silica to improve its wettability and dispersibility with the polymer. The coating has low gloss after film formation, ensuring that it can reflect an excellent matte visual effect. At the same time, it has excellent physical and chemical properties, improves the anti-settling ability of the coating, and enhances the stability of the coating.

[0047] (3) The present invention obtains a resin composition with a suitable particle size distribution and particle size by further optimizing the grinding process during the preparation process, thereby improving the stability of the matting agent in the back coating layer, ensuring that the matte visual effect can be better reflected, and at the same time further improving the coating strength. DETAILED DESCRIPTION

[0048] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.

[0049] It should be noted that specific details are described in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in a variety of other ways different from those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0050] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0051] In a first aspect, the present invention provides a resin composition for a back coating of a thermal transfer ribbon, wherein the resin composition for a back coating of a thermal transfer ribbon comprises the following components in parts by weight:

[0052]

[0053] Among them, the high TG value linear non-crystalline polyester resin includes a first modified polyester resin and a second modified polyester resin in a mass ratio of (2 to 8): (0 to 3); the first modified polyester resin has a B-type structure; the second modified polyester resin has an L-type structure; and the TG value of the high TG value linear non-crystalline polyester resin is above 50°C.

[0054] In the present invention, a high TG value linear non-crystalline polyester resin with specific structural parameters is selected and added. The high TG value can ensure that the high temperature generated instantly by the thermal print head during the thermal transfer process does not damage the back coating; the higher molecular weight can ensure the weather resistance of the coating; a certain hydroxyl value can ensure the adhesion to the PET film and has good film-forming properties. Under the mutual coordination of the various components of the present invention, the resin composition of the present invention can further improve the printing performance, ensure that there is no material residue near the print head after continuous printing, and simultaneously meet multiple properties such as high breakdown energy level, high weather resistance, high heat resistance, high film-forming property, high smoothness and low noise performance.

[0055] As an optional embodiment of the present invention, the content of high TG value linear non-crystalline polyester resin is 2 to 15 parts, for example, it can be 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, etc., preferably 3 to 8 parts, and more preferably 3.9 to 7.5 parts.

[0056] As an optional embodiment of the present invention, the high TG value linear non-crystalline polyester resin comprises a first modified polyester resin and a second modified polyester resin in a mass ratio of (2 to 8): (0 to 3);

[0057] Here, “2-8” can be, for example, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, etc.;

[0058] Among them, “0-3” can be, for example, 0, 0.2, 0.4, 0.6, 0.8, 1, 1.2, 1.4, 1.6, 1.8, 2, 2.2, 2.4, 2.6, 2.8, 3, etc.

[0059] It should be noted that the present invention further limits the addition ratio of the high TG value linear non-crystalline polyester resin, thereby further improving the lubricity, anti-puncture ability and strength of the resin composition and avoiding the problem of falling off. Excessive polyester resin will lead to insufficient lubrication of the coating, making it difficult for the thermal transfer carbon to take off the film and easy to break through; too little polyester resin will lead to insufficient strength of the matting agent on the film, causing the coating to fall off during long-term printing.

[0060] As an optional embodiment of the present invention, the content of the silicone-modified acrylate is 1 to 2 parts, for example, 1 part, 1.2 parts, 1.4 parts, 1.6 parts, 1.8 parts, 2 parts, etc., preferably 0.5 to 1.5 parts, and more preferably 1.0 to 1.5 parts.

[0061] It should be noted that the present invention further limits the addition ratio of silicone-modified acrylate to further improve the breakdown energy level, weather resistance, heat resistance, film-forming property, smoothness, and strength to avoid the problem of shedding. If the silicone-modified acrylate is excessive, the bonding strength between the coating, matting agent, and substrate will be insufficient, and powder will fall off during the use of the thermal transfer ribbon, causing damage to the print head; if the silicone-modified acrylate is too little, the coating will have insufficient smoothness, thermal properties, and anti-puncture properties, making it unsuitable for thermal transfer.

[0062] As an optional embodiment of the present invention, the content of the matting agent is 0.5 to 2 parts, for example, it can be 0.5 parts, 0.6 parts, 0.8 parts, 1 part, 1.2 parts, 1.4 parts, 1.6 parts, 1.8 parts, 2 parts, etc., preferably 0.5 to 1.5 parts, and more preferably 0.8 to 1.2 parts.

[0063] It should be noted that the present invention further limits the addition ratio of the matting agent to further ensure the strength and matte effect of the back coating. If the matting agent is excessive, the polyester resin will not be fully wrapped, and the strength of the matting agent in the back coating will be insufficient, resulting in falling off during continuous printing; if the matting agent is too little, the matte effect will be poor.

[0064] As an optional embodiment of the present invention, the content of the solvent is 30 to 100 parts, for example, it can be 30 parts, 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, 42 parts, 44 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts, 80 parts, 85 parts, 90 parts, 95 parts, 100 parts, etc.

[0065] As an optional embodiment of the present invention, the molecular weight of the first modified polyester resin is 8000-12000, for example, it can be 8000, 8500, 9000, 9500, 10000, 10500, 11000, 11500, 12000, etc.

[0066] As an optional embodiment of the present invention, the TG value of the first modified polyester resin is 55-65°C, for example, it can be 55°C, 56°C, 57°C, 58°C, 59°C, 60°C, 61°C, 62°C, 63°C, 64°C, 65°C, etc.

[0067] As an optional embodiment of the present invention, the hydroxyl value of the first modified polyester resin is 6 to 8 KOHmg / g, for example, it can be 6KOHmg / g, 6.2KOHmg / g, 6.4KOHmg / g, 6.6KOHmg / g, 6.8KOHmg / g, 7KOHmg / g, 7.2KOHmg / g, 7.4KOHmg / g, 7.6KOHmg / g, 7.8KOHmg / g, 8KOHmg / g, etc.

[0068] As an optional embodiment of the present invention, the acid value of the first modified polyester resin is 6 to 8 KOHmg / g, for example, it can be 6KOHmg / g, 6.2KOHmg / g, 6.4KOHmg / g, 6.6KOHmg / g, 6.8KOHmg / g, 7KOHmg / g, 7.2KOHmg / g, 7.4KOHmg / g, 7.6KOHmg / g, 7.8KOHmg / g, 8KOHmg / g, etc.

[0069] As a preferred embodiment of the present invention, the first modified polyester resin is modified polyester GK255 resin.

[0070] In the present invention, the modified polyester GK255 resin refers to the GK255 polyester resin of Toyobo, Japan, which has a molecular weight of 10,000, a TG value of 60°C, a B-type structure, a hydroxyl value of 7 KOHmg / g, and an acid value of 7 KOHmg / g.

[0071] As an optional embodiment of the present invention, the molecular weight of the second modified polyester resin is 1000-5000, for example, it can be 1000, 1500, 2000, 2500, 3000, 3500, 4000, 4500, 5000, etc.

[0072] As an optional embodiment of the present invention, the TG value of the second modified polyester resin is 50-55°C, for example, it can be 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, etc.

[0073] As an optional embodiment of the present invention, the hydroxyl value of the second modified polyester resin is 45-55KOHmg / g, for example, it can be 45KOHmg / g, 46KOHmg / g, 47KOHmg / g, 48KOHmg / g, 49KOHmg / g, 50KOHmg / g, 51KOHmg / g, 52KOHmg / g, 53KOHmg / g, 54KOHmg / g, 55KOHmg / g, etc.

[0074] As a preferred embodiment of the present invention, the second modified polyester resin is modified polyester 220 resin.

[0075] In the present invention, the modified polyester 220 resin refers to the 220 polyester resin of Toyobo Co., Ltd. of Japan, which has a molecular weight of 3000, a TG value of 53°C, an L-type structure, and a hydroxyl value of 50KOHmg / g.

[0076] As an optional embodiment of the present invention, the matting agent is gas-phase nano-silica modified by a silane coupling agent.

[0077] As a preferred embodiment of the present invention, the silane coupling agent is KH570.

[0078] In the present invention, the most preferred is KH570 coupling agent modified gas phase nano silica microparticle matting agent, so that the particle surface carries -CH=CH2 group, and the group can polymerize with methyl methacrylate to prepare methyl methacrylate / nano silica composite material. The silica particles with groups improve the anti-settling ability of the coating and enhance the stability of the coating. The wettability and dispersibility of the modified nano silica powder and the polymer in the formula are improved, and the coating has low gloss after film formation, and has excellent physical and chemical properties, and has the function of using thermal transfer ribbon.

[0079] As an optional embodiment of the present invention, the particle size of the gas-phase nano-silica is 30 to 50 nm, for example, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, etc.

[0080] As an optional embodiment of the present invention, the specific surface area of ​​the fumed nano-silicon dioxide is 160 to 200 m 2 / g, for example, it can be 160m 2 / g, 165m 2 / g, 170m 2 / g, 175m 2 / g, 180m 2 / g, 185m 2 / g, 190m 2 / g, 195m 2 / g, 200m 2 / g, etc.

[0081] As an optional embodiment of the present invention, the solvent includes any one of xylene, butanone or toluene, or a combination of at least two of them.

[0082] As a preferred embodiment of the present invention, the solvent is a mixed solution of butanone and toluene, a mixed solution of butanone and xylene, or a mixed solution of butanone, toluene and xylene.

[0083] As a preferred embodiment of the present invention, the mass ratio of xylene, butanone and toluene is (0-4):(1-2):(0-4);

[0084] Among them, the xylene proportion "0-4" can be, for example, 0, 0.001, 0.005, 0.1, 0.2, 0.4, 0.6, 0.8, 1, 1.2, 1.5, 2, 2.5, 3, 3.5, 4, etc.;

[0085] Wherein, the butanone ratio "1-2" may be, for example, 1, 1.2, 1.4, 1.6, 1.8, 2, etc.;

[0086] Among them, the toluene ratio "0-4" can be, for example, 0, 0.001, 0.005, 0.1, 0.2, 0.4, 0.6, 0.8, 1, 1.2, 1.5, 2, 2.5, 3, 3.5, 4, etc.

[0087] As a preferred embodiment of the present invention, the resin composition for thermal transfer ribbon back coating comprises the following components in parts by weight:

[0088]

[0089] Among them, the content of modified polyester GK255 resin is 3.9 to 7.1 parts, for example, it can be 3.9 parts, 4.0 parts, 4.1 parts, 4.2 parts, 4.3 parts, 4.4 parts, 4.5 parts, 4.6 parts, 4.7 parts, 4.8 parts, 4.9 parts, 5.0 parts, 5.1 parts, 5.2 parts, 5.3 parts, 5.4 parts, 5.5 parts, 5.6 parts, 5.7 parts, 5.8 parts, 5.9 parts, 6.0 parts, 6.1 parts, 6.2 parts, 6.3 parts, 6.4 parts, 6.5 parts, 6.6 parts, 6.7 parts, 6.8 parts, 6.9 parts, 7.0 parts, 7.1 parts, etc.

[0090] Among them, the content of modified polyester 220 resin is 0 to 2.6 parts, for example, it can be 0 part, 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part, 1 part, 1.0 part, 1.1 part, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.8 parts, 2.0 parts, 2.2 parts, 2.4 parts, 2.6 parts, etc.

[0091] The content of the silicone-modified acrylate is 1.1 to 1.8 parts, for example, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.7 parts, 1.8 parts, etc.

[0092] Among them, the content of silane coupling agent modified gas phase nano silica is 0.5 to 1.5 parts, for example, it can be 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1 parts, 1.0 parts, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, etc.

[0093] The content of the solvent is 70 to 90 parts, for example, 70 parts, 72 parts, 74 parts, 76 parts, 78 parts, 80 parts, 82 parts, 84 parts, 86 parts, 88 parts, 90 parts, etc.

[0094] In a second aspect, the present invention provides a method for preparing the resin composition for back coating of a thermal transfer ribbon as described in the first aspect, the preparation method comprising the following steps:

[0095] The various raw materials in the resin composition for the back coating of the thermal transfer ribbon are mixed and then ground to obtain the resin composition for the back coating of the thermal transfer ribbon.

[0096] As an optional embodiment of the present invention, the method for preparing the resin composition for back coating of thermal transfer ribbon specifically comprises the following steps:

[0097] Dissolving the high TG value linear non-crystalline polyester resin in a solvent to obtain a resin solution, dispersing a matting agent in the resin solution, and performing a first grinding to obtain a dispersion;

[0098] The dispersion and the organosilicon-modified acrylate are mixed and ground for a second time to obtain the resin composition for back coating of the thermal transfer ribbon.

[0099] As an optional embodiment of the present invention, the first grinding and / or the second grinding is performed using a sand mill.

[0100] It should be noted that due to different processes leading to different particle size distributions, larger particle sizes will also lead to higher printing noise and deviations in matte effects. The present invention further optimizes the grinding method during the preparation process to obtain a resin composition with a suitable particle size distribution and particle size, thereby improving the stability of the matting agent in the back coating, ensuring that the matte visual effect can be better reflected, and at the same time further improving the coating strength. In the grinding process of the back coating of the thermal transfer ribbon with a matte effect, the sand mill is better than the blue mill, while the emulsifier grinding is not suitable for grinding the resin composition for the back coating of the thermal transfer ribbon.

[0101] As an optional embodiment of the present invention, the particle size of the dispersion obtained by the first grinding is less than 2 μm, for example, it can be 2 μm, 1.9 μm, 1.8 μm, 1.7 μm, 1.6 μm, 1.5 μm, 1.4 μm, 1.3 μm, 1.2 μm, 1.1 μm, 1.0 μm, 0.9 μm, 0.8 μm, 0.7 μm, etc.

[0102] As an optional embodiment of the present invention, the particle size of the resin composition obtained by the second grinding is less than 0.6μm, for example, it can be 0.6μm, 0.55μm, 0.5μm, 0.45μm, 0.4μm, 0.35μm, 0.3μm, 0.25μm, 0.2μm, 0.15μm, 0.1μm, 0.05μm, etc.

[0103] In a third aspect, the present invention provides a thermal transfer back coating layer, wherein the thermal transfer back coating layer is formed by curing the resin composition for thermal transfer ribbon back coating as described in the first aspect.

[0104] In a fourth aspect, the present invention provides a method for preparing the thermal transfer back coating as described in the third aspect, the preparation method comprising the following steps:

[0105] The resin composition for thermal transfer ribbon back coating as described in the first aspect is coated on the surface of the substrate and cured by baking to obtain the thermal transfer back coating.

[0106] As an optional embodiment of the present invention, the coating amount of the resin composition for the back coating of the thermal transfer ribbon is 0.2 to 0.4 g / m 2 , for example, it can be 0.2g / m 2, 0.22g / m 2 , 0.24g / m 2 , 0.26g / m 2 , 0.28g / m 2 , 0.3g / m 2 , 0.32g / m 2 , 0.34g / m 2 , 0.36g / m 2 , 0.38g / m 2 , 0.4g / m 2 , 0.42g / m 2 , 0.44g / m 2 , 0.46g / m 2 , 0.48g / m 2 , 0.5g / m 2 wait.

[0107] As a preferred embodiment of the present invention, the coating amount of the resin composition for the back coating of the thermal transfer ribbon is 0.25 to 0.35 g / m 2 .

[0108] As an optional embodiment of the present invention, the baking temperature is 50-60°C, for example, it can be 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C, 60°C, etc.

[0109] As an optional implementation manner of the present invention, the baking time is 5 to 9 seconds, for example, it can be 5 seconds, 5.5 seconds, 6 seconds, 6.5 seconds, 7 seconds, 7.5 seconds, 8 seconds, 8.5 seconds, 9 seconds, etc.

[0110] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.

[0111] The sources of raw materials and their parameters in the following examples and comparative examples are as follows:

[0112]

[0113] Examples 1 to 8

[0114] Embodiments 1 to 8 provide resin compositions for thermal transfer ribbon back coating in different formulation ratios, wherein the resin compositions for thermal transfer ribbon back coating include the following components in parts by weight:

[0115]

[0116] Wherein, the mixed solvent consists of xylene and butanone in a mass ratio of 2:1.

[0117] The resin composition for the back coating of the thermal transfer ribbon in this embodiment is prepared by the following steps:

[0118] First, dissolve GK255 resin and 220 resin in a mixed solvent, then evenly disperse KH570 modified gas phase nano-silica therein, and grind it twice using a sand mill (the average particle size is below 2 μm); then add and evenly disperse the organosilicon-modified acrylate, and continue to grind it using a sand mill until the average particle size is less than 0.6 μm, to obtain the resin composition for the back coating of the thermal transfer ribbon.

[0119] Example 9

[0120] This embodiment provides a resin composition for back coating of a thermal transfer ribbon, which is different from Embodiment 1 only in that an emulsifier is used for grinding during the preparation process.

[0121] Example 10

[0122] This embodiment provides a resin composition for back coating of a thermal transfer ribbon, which is different from Embodiment 1 only in that a blue grinder is used for grinding during the preparation process.

[0123] Comparative Examples 1 to 11

[0124] Comparative Examples 1 to 11 provide different formulation ratios for a resin composition, wherein the resin composition comprises the following components in parts by weight:

[0125]

[0126]

[0127] Wherein, the mixed solvent consists of xylene and butanone in a mass ratio of 2:1.

[0128] The preparation method of the resin composition of this comparative example is consistent with that of Example 1.

[0129] Comparative Example 12

[0130] This comparative example provides a resin composition, which is different from Example 1 only in that GK255 resin is not added, the content of 220 resin is increased to 7.2 parts, and the contents of other components and the preparation method are completely consistent with Example 1.

[0131] Comparative Example 13

[0132] This comparative example provides a resin composition, which is different from Example 1 only in that 7.2 parts of 240 resin are added instead of GK255 resin and 220 resin, and the contents of other components and the preparation method are completely consistent with those of Example 1.

[0133] Comparative Example 14

[0134] This comparative example provides a resin composition, which is different from Example 1 only in that 7.2 parts of 270 resin are added instead of GK255 resin and 220 resin, and the contents of other components and the preparation method are completely consistent with those of Example 1.

[0135] Test Example 1

[0136] Back coating evaluation index test

[0137] Test samples: the resin compositions for back coating of thermal transfer ribbons provided in Examples 1 to 8, and the resin compositions provided in Comparative Examples 1 to 14;

[0138] Test method:

[0139] The industrial machine Zebra 105SL PLUS-2 model is the model with the largest number of shares in the market. Its printing speed can be set from 1 inch per second to 8 inches per second, and the energy level can be set from 1 to 30. Generally, the printing speed is set from 4 to 6 inches per second, and the energy level is generally set from 10 to 20.

[0140] The evaluation index standards for the matte back coating of thermal transfer ribbons are as follows:

[0141] (1) Printing

[0142] The printing conditions mainly examine whether there are more than 4 energy level windows with clear transfer at a speed of 4 inches per second to 6 inches per second for 0° barcode, 90° barcode, black block, character, pattern, etc.

[0143] (2) Continuous printing

[0144] Continuous printing is generally performed at a speed of 4 inches per second to 6 inches per second and an energy level of 14-18. Print continuously for 200-300 meters and check whether there is any material residue near the print head or the print head.

[0145] (3) Highest breakdown energy level

[0146] The breakdown energy level mainly reflects the heat resistance of the thermal transfer back coating. Generally, the speed is 4 inches per second, and the energy level is gradually increased until it reaches 30 (highest) energy level to check whether the thermal transfer ribbon is damaged. The breakdown of the ribbon is likely to cause the print head to break and damage the needle.

[0147] (4) Thermal performance

[0148] Thermal performance mainly reflects the isolation performance of the thermal transfer ribbon; place the ribbon in a 55±1℃ oven for 20 hours, take it out and let it stand for 2 hours, rewind it quickly, and check whether there is any anti-sticking phenomenon of the thermal transfer coating.

[0149] (5) Glossiness

[0150] The glossiness of the matte effect is tested by a gloss meter (60° angle). A glossiness between 20-40 (60° angle) can reflect an excellent matte visual effect.

[0151] (6) Printing noise

[0152] Printing noise is measured by a digital noise meter (AS-K8) with the probe about 3cm away from the print head; generally, decibel values ​​below 80db are not considered harmful noise. Thermal transfer printers are office supplies, and printing noise is the most important aspect of inspection besides print quality.

[0153] Printing conditions, continuous printing, high energy level without breakdown, and thermal performance are the basic functional requirements for back coating and must be met; matte effect is an appearance requirement, and printing noise is a high-quality requirement and needs to be met as much as possible.

[0154] The test results are shown in Tables 1 and 2 below:

[0155] Table 1

[0156]

[0157]

[0158] As shown in Table 1, the resin composition for thermal transfer ribbon back coating prepared in Examples 1 to 5 of the present invention ensures excellent printing performance by adding GK255 resin, ensures that there is no material residue near the print head after continuous printing, and simultaneously satisfies multiple performances such as high breakdown energy level, high weather resistance, high heat resistance, high film forming property, high smoothness and low noise performance. The fumed nano-silica modified by a specific matting agent silane coupling agent improves its wettability and dispersibility with the polymer, and the coating has low gloss after film formation, ensuring that it can reflect an excellent matte visual effect, and at the same time has excellent physical and chemical properties, improves the anti-settling ability of the coating, and enhances the stability of the coating.

[0159] From the samples of Comparative Examples 1 and 2, it can be seen that too much silicone-modified acrylate will cause problems in the quality of the printed mark. From the samples provided by Comparative Examples 3 and 4, it can be seen that the silicone-modified acrylate is insufficient, and the polyester resin does not meet the requirements of thermal transfer in terms of heat insulation and smoothness. GK255 resin has improved printing noise, but lacks in bonding strength. 220 resin has good bonding between matting powder and silicone-modified acrylate, but lacks in printing noise.

[0160] Therefore, experiments show that excessive matting agent will lead to insufficient wrapping of polyester resin, insufficient strength of matting agent in the back coating, and cause it to fall off during continuous printing; too little matting agent will lead to poor matte effect. Experiments show that excessive polyester resin will lead to insufficient lubrication of the coating, making it difficult for the thermal transfer carbon ribbon to remove the film and easy to penetrate; too little polyester resin will lead to insufficient strength of the matting agent on the film, causing the coating to fall off during long-term printing. Experiments show that excessive silicone-modified acrylate will lead to insufficient bonding strength between the coating, matting agent, and substrate, and powder will fall off during the use of the thermal transfer ribbon, causing damage to the print head; too little silicone-modified acrylate will lead to insufficient smoothness, thermal properties, and anti-puncture properties of the coating, making it unsuitable for thermal transfer use.

[0161] As shown in Comparative Examples 6 to 11, the increase in the solid content of silicone-modified acrylate can appropriately reduce printing noise, and GK255 resin mixed with 220 resin can also adapt to reducing printing noise.

[0162] From the samples provided by Comparative Examples 12 to 14, although Comparative Example 6 only uses 220 resin for continuous printing and is qualified, when the energy level is increased to 30, the thermal transfer ribbon is damaged. Comparative Example 7 only uses 240 resin, and there will be white residue on the print head and near the print head after continuous printing of 200 meters, and the thermal transfer color will be punctured and damaged at 24 energy levels. Comparative Example 8 only uses 270 resin, and there will be slight residue on the print head and near the print head after continuous printing of 200 meters. It can be seen that Japan's Toyobo 220 and SKYBON's GK255 can meet the back coating requirements of thermal transfer carbon ribbons.

[0163] Table 2

[0164]

[0165]

[0166] As shown in Table 2, different processes will lead to different particle size distributions. Larger particle sizes will also lead to higher printing noise and a deviation in matte effect. The coating amount of matte back coating is 0.2-0.4 g / m 2 The smaller the matting agent particle size, the more stable the matting agent is in the back coating and the lower the glossiness. Experimental verification shows that the coating strength is better when the particle size is less than 2μm. Therefore, it can be concluded that the sand mill is better than the blue mill in the grinding process of the back coating of the thermal transfer ribbon with matte effect, and the emulsifier grinding process is not suitable.

[0167] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A resin composition for back coating of thermal transfer ribbon, characterized in that: The resin composition for back coating of thermal transfer ribbon comprises the following components in parts by weight: Among them, the high TG value linear non-crystalline polyester resin includes a first modified polyester resin and a second modified polyester resin in a mass ratio of (2 to 8): (0 to 3); the first modified polyester resin has a B-type structure; the second modified polyester resin has an L-type structure; and the TG value of the high TG value linear non-crystalline polyester resin is above 50°C.

2. The resin composition for back coating of thermal transfer ribbon according to claim 1, characterized in that: The molecular weight of the first modified polyester resin is 8000 to 12000; and / or, the TG value of the first modified polyester resin is 55 to 65° C.; and / or, the hydroxyl value of the first modified polyester resin is 6 to 8 KOHmg / g; and / or, the acid value of the first modified polyester resin is 6 to 8 KOHmg / g; Preferably, the first modified polyester resin is modified polyester GK255 resin.

3. The resin composition for thermal transfer ribbon back coating according to claim 1, characterized in that: The molecular weight of the second modified polyester resin is 1000 to 5000; and / or, the TG value of the second modified polyester resin is 50-55° C.; and / or, the hydroxyl value of the second modified polyester resin is 45 to 55 KOHmg / g; Preferably, the second modified polyester resin is modified polyester 220 resin.

4. The resin composition for back coating of thermal transfer ribbon according to claim 1, characterized in that: The matting agent is gas-phase nano-silica modified by a silane coupling agent; Preferably, the silane coupling agent is KH570; Preferably, the particle size of the fumed nano-silicon dioxide is 30 to 50 nm; Preferably, the specific surface area of ​​the fumed nano-silicon dioxide is 160 to 200 m 2 / g; Preferably, the solvent comprises any one of xylene, butanone or toluene, or a combination of at least two thereof, preferably a mixed solution of butanone and toluene, a mixed solution of butanone and xylene, or a mixed solution of butanone, toluene and xylene; Preferably, the mass ratio of xylene, butanone and toluene is (0-4):(1-2):(0-4).

5. The resin composition for back coating of thermal transfer ribbon according to claim 1, characterized in that: The resin composition for back coating of thermal transfer ribbon comprises the following components in parts by weight:

6. A method for preparing a resin composition for back coating of a thermal transfer ribbon according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: The various raw materials in the resin composition for the back coating of the thermal transfer ribbon are mixed and then ground to obtain the resin composition for the back coating of the thermal transfer ribbon.

7. The method for preparing the resin composition for back coating of thermal transfer ribbon according to claim 6, characterized in that: The preparation method specifically comprises the following steps: Dissolving the high TG value linear non-crystalline polyester resin in a solvent to obtain a resin solution, dispersing a matting agent in the resin solution, and performing a first grinding to obtain a dispersion; The dispersion and the organosilicon-modified acrylate are mixed and ground for a second time to obtain the resin composition for back coating of the thermal transfer ribbon; Preferably, the first grinding and / or the second grinding is performed using a sand mill; Preferably, the particle size of the dispersion obtained by the first grinding is less than 2 μm; Preferably, the particle size of the resin composition obtained by the second grinding is less than 0.6 μm.

8. A thermal transfer back coating, characterized in that: The thermal transfer back coating layer is formed by curing the resin composition for thermal transfer ribbon back coating according to any one of claims 1 to 5.

9. A method for preparing a thermal transfer back coating according to claim 8, characterized in that: The preparation method comprises the following steps: The resin composition for thermal transfer ribbon back coating according to any one of claims 1 to 5 is applied to the surface of a substrate and cured by baking to obtain the thermal transfer back coating.

10. The method for preparing a thermal transfer back coating according to claim 9, characterized in that: The coating amount of the resin composition for the back coating of the thermal transfer ribbon is 0.2 to 0.4 g / m 2 ; Preferably, the baking temperature is 50-60°C; Preferably, the baking time is 5 to 9 seconds.

Citation Information

Patent Citations

  • Thermal transfer ribbon used for edge crush type printer and preparation method thereof

    CN102653189A

  • Silicon-containing acrylate-polyester resin, and finish coat and application thereof

    CN102850536A

  • Organic silicon modified acrylic resin as well as preparation method and application thereof

    CN118290669A

  • Thermal transfer printing recording medium and image forming method

    CN1291551A

  • Ink ribbon for thermal transfer recording

    JP1994079978A