Stone-like coating as well as preparation method and construction process thereof
Through the combination of component A, component B and component C and the simplification of the construction technology, the problems of complex construction technology and poor coating performance of imitation limestone coatings are solved, and the thin and flat coating effect and long-term stability are achieved, which is in line with the Industry standards.
Patent Information
- Application Number
- CN202411131173.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-17
- Publication Date
- 2024-11-08
AI Technical Summary
The existing construction process of imitation limestone paint consumes a lot of materials and is complex, resulting in poor flexibility, water resistance and weather resistance of the coating, easy to damage and short service life.
By simplifying the construction process and thin layer spraying technology, high-quality silicon polymers and preservatives are used to form a light and flat paint film to improve the weather resistance of the coating. Water and alkali resistance and long-term stability of the coating is ensured through specific construction steps.
It achieves a thin and flat coating effect, extends the service life of the coating, improves the weather resistance, water resistance and alkali resistance of the coating, complies with the JC/T24-2018 industry standards, simplifies the construction process and reduces the materials Consumption.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of stone-like paint and a preparation method and a construction process thereof, and in particular to a stone-like paint and a preparation method and a construction process thereof. Background Art
[0002] As a natural stone, limestone is widely used in modern architectural decoration. However, due to its own weight, limestone has a high risk of falling off after a long period of use. In addition, as a natural stone, excessive mining of limestone will lead to problems such as mineral resource depletion and environmental pollution. Therefore, imitation limestone paint came into being and occupied a place in the architectural paint market. As the application of imitation limestone paint becomes more and more widespread, many problems are also exposed.
[0003] The existing imitation limestone coating needs to be sprayed with a thicker coating, which results in the inability to restore the effect of natural stone; secondly, the existing imitation limestone coating construction process is relatively material-consuming and complex; secondly, in order to achieve better polishing construction performance, the existing process often reduces the emulsion content of the imitation limestone coating or increases the amount of filler, so that the emulsion's wrapping of the filler becomes worse (the worse the emulsion's wrapping of the filler, the better the polishing performance, and vice versa), resulting in the coating's flexibility, water resistance, and weather resistance becoming worse, and easy to powderize, resulting in the coating being easily damaged and faded in harsh climates; and reducing the coating's service life;
[0004] Therefore, it is urgent to develop a kind of imitation stone coating and its preparation method and construction process to solve the above-mentioned problems. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the defects of the above-mentioned technology and provide a stone-like paint and a preparation method and a construction process thereof; after the stone-like paint provided by the present invention is applied, a thin, flat and smooth paint film is obtained, which better restores the effect of natural stone, has no dust pollution during construction, and also has excellent weather resistance, water resistance, alkali resistance, flexibility, is not easy to fade, has a long service life of the coating, and the performance indicators meet the requirements of the JC / T24-2018 industry standard.
[0006] In order to solve the above technical problems, the technical solution provided by the present invention is a stone-like paint: comprising component A, component B and component C;
[0007] The component A comprises the following components in weight percentage: 88-108 parts of purified water, 0.2-0.4 parts of suspending agent, 0.5-0.9 parts of preservative, and 0.8-1.2 parts of isolating agent;
[0008] The component B comprises the following components in weight percentage: 60-80 parts of purified water, 15-25 parts of silicone polymer, 0.4-0.6 parts of cellulose ether, 4-6 parts of titanium dioxide, 0.4-0.6 parts of defoaming agent, 0.1-0.3 parts of dispersant, 0.6-1 parts of diol, 2-3 parts of film-forming aid, and 0.4-0.6 parts of preservative;
[0009] The component C comprises the following components in weight percentage: 15-25 parts of purified water, 60-80 parts of silicone polymer, 0.8-1.2 parts of preservative, 4-6 parts of film-forming aid, 2-4 parts of diol, and 0.8-1.2 parts of thickener;
[0010] The mass ratio of component A, component B and component C is 3:5:2.
[0011] As an improvement, the component A includes the following components in weight percentage: 98 parts of purified water, 0.3 parts of suspending agent, 0.7 parts of preservative, and 1 part of isolating agent;
[0012] The component B comprises the following components in weight percentage: 70 parts of purified water, 20 parts of silicone polymer, 0.5 parts of cellulose ether, 5 parts of titanium dioxide, 0.5 parts of defoaming agent, 0.2 parts of dispersant, 0.8 parts of diol, 2.5 parts of film-forming aid, and 0.5 parts of preservative;
[0013] The component C comprises the following components in weight percentage: 20 parts of pure water, 70 parts of silicone polymer, 1 part of preservative, 5 parts of film-forming aid, 23 parts of diol, and 1 part of thickener.
[0014] The present invention provides a method for preparing the above-mentioned stone-like coating, comprising the following steps:
[0015] The first step is to mix the components of component A, component B and component C evenly;
[0016] Step 2: Pour 5 parts of the mixed B component into 3 parts of the mixed A component, mix them thoroughly and separate them;
[0017] The third step is to add 2 parts of the mixed C component to the solvent obtained in the second step, mix them evenly, and obtain the stone-like paint.
[0018] The present invention provides a construction process for the above-mentioned stone-like coating, which is characterized by comprising the following steps:
[0019] Step 1, a base layer: apply multiple coats of putty on the rough cement base for leveling, and then further sand it until it is completely flat and has no traces of neat walls; then use a polymer penetrating coating to seal the putty layer, and use two coats of roller coating to isolate the base layer;
[0020] Step 2, two middle layers: Spray the lime base color as the material, and spray two layers to achieve complete coloring; after the two layers of spraying are dry, lightly sand the sprayed lime base until the lime base is flat and free of particles; then spray the imitation stone paint on the sanded lime base, spray it in two thin sprays, and dry it;
[0021] The third step, three layers of surface: use high-quality specially formulated polymer surface imitation stone paint as the construction material, and use spraying technology to protect the surface layer. Spray twice, use atmospheric pressure and strong atomization to achieve a thicker spray without sagging, ensure the thickness of the surface layer to provide protection, make it better resistant to water and stains, and extend the life of the coating.
[0022] The advantages of the present invention compared with the prior art are:
[0023] 1. Get rid of the high consumables and complex process of conventional stone-like coatings, and use a simpler way to simplify the construction process and time. The extremely low consumables per square meter can greatly shorten the construction period;
[0024] 2. The coating after application is thinner, more transparent, and highly restores the effect of natural stone;
[0025] 3. On the basis of a thin coating, high-quality silicone polymer is used as the main body to restore the stone simulation effect while satisfying its weather resistance, water resistance and alkali resistance. The wrapping of silicone polymer chain segments can make the coating less likely to be damaged or faded under the harsh climate of the exterior wall, and it is more solid and flexible, which increases the service life of the coating and maintains its beauty all year round. DETAILED DESCRIPTION
[0026] The following is a further detailed description of a stone-like coating and a preparation method and construction process of the present invention in conjunction with embodiments.
[0027] A stone-like paint comprises a component A, a component B and a component C;
[0028] Component A includes the following components in weight percentage:
[0029] 88-108 parts of purified water
[0030] Suspending agent 0.2-0.4 parts
[0031] Preservative 0.5-0.9 parts
[0032] Release agent 0.8-1.2 parts;
[0033] Component B includes the following components in weight percentage:
[0034] 60-80 parts of purified water
[0035] 15-25 parts of silicone polymer
[0036] Cellulose ether 0.4-0.6 parts
[0037] 4-6 parts of titanium dioxide
[0038] Defoamer 0.4-0.6 parts
[0039] Dispersant 0.1-0.3 parts
[0040] 0.6-1 part of diol
[0041] 2-3 parts of film-forming aid
[0042] Preservative 0.4-0.6 parts;
[0043] Component C includes the following components in weight percentage:
[0044] 15-25 parts of purified water
[0045] 60-80 parts of silicone polymer
[0046] Preservative 0.8-1.2 parts
[0047] 4-6 parts of film-forming aid
[0048] 2-4 parts of diol
[0049] Thickener 0.8-1.2 parts;
[0050] The mass ratio of component A, component B and component C is 3:5:2.
[0051] A method for preparing a stone-like coating, characterized in that:
[0052] The first step is to mix the components of component A, component B and component C evenly;
[0053] Step 2: Pour 5 parts of the mixed B component into 3 parts of the mixed A component, mix them thoroughly and separate them;
[0054] The third step is to add 2 parts of the mixed C component to the solvent obtained in the second step, mix them evenly, and obtain the stone-like paint.
[0055] A construction process of imitation stone coating, characterized in that it comprises the following steps:
[0056] Step 1, a base layer: apply multiple coats of putty on the rough cement base for leveling, and then further sand it until it is completely flat and has no traces of neat walls; then use a polymer penetrating coating to seal the putty layer, and use two coats of roller coating to isolate the base layer;
[0057] Step 2, two middle layers: Spray the lime base color as the material, and spray two layers to achieve complete coloring; after the two layers of spraying are dry, lightly sand the sprayed lime base until the lime base is flat and free of particles; then spray the imitation stone paint on the sanded lime base, spray it in two thin sprays, and dry it;
[0058] The third step, three layers of surface: use high-quality specially formulated polymer surface imitation stone paint as the construction material, and use spraying technology to protect the surface layer. Spray twice, use atmospheric pressure and strong atomization to achieve a thicker spray without sagging, ensure the thickness of the surface layer to provide protection, make it better resistant to water and stains, and extend the life of the coating.
[0059] When the present invention is implemented,
[0060] Embodiment 1,
[0061] Preparation of imitation stone coating: First, take component A: 88 parts of pure water, 0.2 parts of suspending agent, 0.5 parts of preservative, and 0.8 parts of release agent;
[0062] Component B: 60 parts of purified water, 15 parts of silicone polymer, 0.4 parts of cellulose ether, 4 parts of titanium dioxide, 0.4 parts of defoaming agent, 0.1 parts of dispersant, 0.6 parts of diol, 2 parts of film-forming aid, 0.4 parts of preservative;
[0063] Component C: 15 parts of purified water, 60 parts of silicone polymer, 0.8 parts of preservative, 4 parts of film-forming aid, 2 parts of diol, 0.8 parts of thickener;
[0064] Step 2: Pour 5 parts of the mixed B component into 3 parts of the mixed A component, mix them thoroughly and separate them;
[0065] The third step is to add 2 parts of the mixed C component to the solvent obtained in the second step, mix them evenly, and obtain the stone-like paint.
[0066] The construction process of the imitation stone coating is characterized by comprising the following steps:
[0067] Step 1, a base layer: apply multiple coats of putty on the rough cement base for leveling, and then further sand it until it is completely flat and has no traces of neat walls; then use a polymer penetrating coating to seal the putty layer, and use two coats of roller coating to isolate the base layer;
[0068] Step 2, two middle layers: Spray the lime base color as the material, and spray two layers to achieve complete coloring; after the two layers of spraying are dry, lightly sand the sprayed lime base until the lime base is flat and free of particles; then spray the imitation stone paint on the sanded lime base, spray it in two thin sprays, and dry it;
[0069] The third step, three layers of surface: use high-quality specially formulated polymer surface imitation stone paint as the construction material, and use spraying technology to protect the surface layer. Spray twice, use atmospheric pressure and strong atomization to achieve a thicker spray without sagging, ensure the thickness of the surface layer to provide protection, make it better resistant to water and stains, and extend the life of the coating.
[0070] Embodiment 2:
[0071] Preparation of imitation stone coating: First, take component A: 98 parts of purified water, 0.3 parts of suspending agent, 0.7 parts of preservative, and 1 part of release agent;
[0072] Component B: 70 parts of purified water, 20 parts of silicone polymer, 0.5 parts of cellulose ether, 5 parts of titanium dioxide, 0.5 parts of defoaming agent, 0.2 parts of dispersant, 0.8 parts of diol, 2.5 parts of film-forming aid, 0.5 parts of preservative;
[0073] Component C: 20 parts of purified water, 70 parts of silicone polymer, 1 part of preservative, 5 parts of film-forming aid, 23 parts of diol, 1 part of thickener;
[0074] Step 2: Pour 5 parts of the mixed B component into 3 parts of the mixed A component, mix them thoroughly and separate them;
[0075] The third step is to add 2 parts of the mixed C component to the solvent obtained in the second step, mix them evenly, and obtain the stone-like paint;
[0076] The construction process of the imitation stone coating is characterized by comprising the following steps:
[0077] Step 1, a base layer: apply multiple coats of putty on the rough cement base for leveling, and then further sand it until it is completely flat and has no traces of neat walls; then use a polymer penetrating coating to seal the putty layer, and use two coats of roller coating to isolate the base layer;
[0078] Step 2, two middle layers: Spray the lime base color as the material, and spray two layers to achieve complete coloring; after the two layers of spraying are dry, lightly sand the sprayed lime base until the lime base is flat and free of particles; then spray the imitation stone paint on the sanded lime base, spray it in two thin sprays, and dry it;
[0079] The third step, three layers of surface: use high-quality specially formulated polymer surface imitation stone paint as the construction material, and use spraying technology to protect the surface layer. Spray twice, use atmospheric pressure and strong atomization to achieve a thicker spray without sagging, ensure the thickness of the surface layer to provide protection, make it better resistant to water and stains, and extend the life of the coating.
[0080] Embodiment 3,
[0081] Preparation of imitation stone coating: First, take component A: 108 parts of pure water, 0.4 parts of suspending agent, 0.9 parts of preservative, and 1.2 parts of release agent;
[0082] Component B: 80 parts of purified water, 25 parts of silicone polymer, 0.6 parts of cellulose ether, 6 parts of titanium dioxide, 0.6 parts of defoaming agent, 0.3 parts of dispersant, 1 part of diol, 3 parts of film-forming aid, 0.6 parts of preservative;
[0083] Component C: 25 parts of purified water, 80 parts of silicone polymer, 1.2 parts of preservative, 6 parts of film-forming aid, 4 parts of diol, and 1.2 parts of thickener.
[0084] Step 2: Pour 5 parts of the mixed B component into 3 parts of the mixed A component, mix them thoroughly and separate them;
[0085] The third step is to add 2 parts of the mixed C component to the solvent obtained in the second step, mix them evenly, and obtain the stone-like paint;
[0086] The construction process of the imitation stone coating is characterized by comprising the following steps:
[0087] Step 1, a base layer: apply multiple coats of putty on the rough cement base for leveling, and then further sand it until it is completely flat and has no traces of neat walls; then use a polymer penetrating coating to seal the putty layer, and use two coats of roller coating to isolate the base layer;
[0088] Step 2, two middle layers: Spray the lime base color as the material, and spray two layers to achieve complete coloring; after the two layers of spraying are dry, lightly sand the sprayed lime base until the lime base is flat and free of particles; then spray the imitation stone paint on the sanded lime base, spray it in two thin sprays, and dry it;
[0089] The third step, three layers of surface: use high-quality specially formulated polymer surface imitation stone paint as the construction material, and use spraying technology to protect the surface layer. Spray twice, use atmospheric pressure and strong atomization to achieve a thicker spray without sagging, ensure the thickness of the surface layer to provide protection, make it better resistant to water and stains, and extend the life of the coating.
[0090] This paint is a stone-like decorative paint and is not primarily functional; however, the materials are selected to ensure a better service life. Combined with standard base and surface layer construction, the final coating can guarantee a long-term initial effect.
[0091] The present invention and its embodiments are described above, and such description is not restrictive. What is described in the embodiment is only one of the embodiments of the present invention, and is not actually limited thereto. In short, if ordinary technicians in the field are inspired by it, without departing from the purpose of the invention, and without creatively designing methods and embodiments similar to the technical solution, they should all fall within the protection scope of the present invention.
Claims
1. A stone-like paint, characterized in that: It includes component A, component B and component C; The component A comprises the following components in weight percentage: 88-108 parts of purified water, 0.2-0.4 parts of suspending agent, 0.5-0.9 parts of preservative, and 0.8-1.2 parts of isolating agent; The component B comprises the following components in weight percentage: 60-80 parts of purified water, 15-25 parts of silicone polymer, 0.4-0.6 parts of cellulose ether, 4-6 parts of titanium dioxide, 0.4-0.6 parts of defoaming agent, 0.1-0.3 parts of dispersant, 0.6-1 parts of diol, 2-3 parts of film-forming aid, and 0.4-0.6 parts of preservative; The component C comprises the following components in weight percentage: 15-25 parts of purified water, 60-80 parts of silicone polymer, 0.8-1.2 parts of preservative, 4-6 parts of film-forming aid, 2-4 parts of diol, and 0.8-1.2 parts of thickener; The mass ratio of component A, component B and component C is 3:5:
2.
2. The stone-like paint according to claim 1, characterized in that: The component A comprises the following components in weight percentage: 88 parts of purified water, 0.2 parts of suspending agent, 0.5 parts of preservative, and 0.8 parts of isolating agent; The component B includes the following components in weight percentage: 60 parts of purified water, 15 parts of silicone polymer, 0.4 parts of cellulose ether, 4 parts of titanium dioxide, 0.4 parts of defoaming agent, 0.1 parts of dispersant, 0.6 parts of diol, 2 parts of film-forming aid, and 0.4 parts of preservative; The component C comprises the following components in weight percentage: 15 parts of purified water, 60 parts of silicone polymer, 0.8 parts of preservative, 4 parts of film-forming aid, 2 parts of diol, and 0.8 parts of thickener.
3. The stone-like paint according to claim 1, characterized in that: The component A comprises the following components in weight percentage: 98 parts of purified water, 0.3 parts of suspending agent, 0.7 parts of preservative, and 1 part of isolating agent; The component B comprises the following components in weight percentage: 70 parts of purified water, 20 parts of silicone polymer, 0.5 parts of cellulose ether, 5 parts of titanium dioxide, 0.5 parts of defoaming agent, 0.2 parts of dispersant, 0.8 parts of diol, 2.5 parts of film-forming aid, and 0.5 parts of preservative; The component C comprises the following components in weight percentage: 20 parts of pure water, 70 parts of silicone polymer, 1 part of preservative, 5 parts of film-forming aid, 23 parts of diol, and 1 part of thickener.
4. The stone-like paint according to claim 1, characterized in that: The component A comprises the following components in weight percentage: 108 parts of purified water, 0.4 parts of suspending agent, 0.9 parts of preservative, and 1.2 parts of isolating agent; The component B comprises the following components in weight percentage: 80 parts of purified water, 25 parts of silicone polymer, 0.6 parts of cellulose ether, 6 parts of titanium dioxide, 0.6 parts of defoamer, 0.3 parts of dispersant, 1 part of diol, 3 parts of film-forming aid, and 0.6 parts of preservative; The component C includes the following components in weight percentage: 25 parts of purified water, 80 parts of silicone polymer, 1.2 parts of preservative, 6 parts of film-forming aid, 4 parts of diol, and 1.2 parts of thickener.
5. A method for preparing the stone-like coating according to any one of claims 1 to 4, characterized in that: The first step is to mix the components of component A, component B and component C evenly; Step 2: Pour 5 parts of the mixed B component into 3 parts of the mixed A component, mix them thoroughly and separate them; The third step is to add 2 parts of the mixed C component to the solvent obtained in the second step, mix them evenly, and obtain the stone-like paint.
6. A construction process using the stone-like paint according to any one of claims 1 to 4, characterized in that: The following steps are included: Step 1, a base layer: apply multiple coats of putty on the rough cement base for leveling, and then further sand it until it is completely flat and has no traces of neat walls; then use a polymer penetrating coating to seal the putty layer, and use two coats of roller coating to isolate the base layer; Step 2, two middle layers: Spray the lime base color as the material, and spray two layers to achieve complete coloring; after the two layers of spraying are dry, lightly sand the sprayed lime base until the lime base is flat and free of particles; then spray the imitation stone paint on the sanded lime base, spray it in two thin sprays, and dry it; The third step, three surface layers: Use high-quality specially formulated polymer surface layer materials as construction materials, and use spraying technology to protect the surface layer. Spray twice, use atmospheric pressure and strong atomization to achieve thicker spraying without sagging, ensure the thickness of the surface layer to provide protection, make it better resistant to water and stains, and extend the life of the coating.
Citation Information
Patent Citations
Method for manufacturing composite type imitation marble coating by colorful stone-like paint
CN111364710A
Limestone-like multicolor paint and construction method thereof
CN111484781A
Imitation stone paint coating structure
CN209096368U