EPE packaging adhesive film for multi-layer photovoltaic module

By using carbodiimide or carboyldiimide compounds and aminosilane coupling agent in the encapsulation film of photovoltaic modules, the PID effect and interlayer adhesion of photovoltaic modules in the humid and heat environment are solved. The problem of insufficient synergy achieves higher anti-PID effect and light transmittance maintenance.

CN118909555APending Publication Date: 2024-11-08SHAOXING HUAYUAN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411247456.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing photovoltaic module packaging film cannot effectively prevent potential-induced attenuation (PID) effects in humid and heat environments, and due to insufficient adhesion between materials, there is a risk of interlayer separation and delamination, which affects the long-term stability of the components and Light transmittance.

Method used

Using a multi-layer photovoltaic module EPE encapsulation film, including a polyolefin layer and an EVA layer distributed on both sides, carbodiimide or carboyldiimide compounds are added as acid remover A, and silane couples with amino groups As acid remover B, the coupling agent enhances interface adhesion in a humid and heat environment through the reactive acid remover system and prevents interlayer separation.

Benefits of technology

It significantly improves the PID effect and interlayer adhesion of photovoltaic modules in humid and heat environments, maintains light transmittance, and maintains the interlayer peeling intensity after a long period of use, significantly reducing the power attenuation of the PID effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005031220550000131
    Figure BDA0005031220550000131
  • Figure BDA0005031220550000141
    Figure BDA0005031220550000141
Patent Text Reader

Abstract

The invention discloses an EPE packaging adhesive film for a multilayer photovoltaic module. The EPE packaging adhesive film comprises a polyolefin layer and EVA layers distributed on the two sides of the polyolefin layer. The main body material of the polyolefin layer is a polyolefin material, and the main body resin of the EVA layer is EVA resin; according to the weight ratio, the EVA layer further comprises 0.01-1% of a deacidification agent A and 0.1-5% of a catalyst relative to the weight of the deacidification agent A; the polyolefin layer also comprises 0.01-1% of a deacidification agent B; the acid removal agent A is carbodiimide or a carbodiimide compound; the deacidification agent B is a silane coupling agent with amino groups. According to the packaging adhesive film, a reaction type acid remover system is adopted, the packaging adhesive film can be better applied to a humid and hot environment, a better anti-PID effect is achieved, the light transmittance is not affected, and the interface adhesive force between layers can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photovoltaic module encapsulation films, and in particular to a multi-layer photovoltaic module EPE encapsulation film. Background Art

[0002] Photovoltaics is developing very fast, and battery technology is also rapidly iterating, from PERC to TOPCON, HJT, perovskite and other technical routes. As batteries advance, they are becoming more and more sensitive to water vapor, and the original packaging materials will not be able to meet the requirements of existing battery technology.

[0003] The original packaging film is generally a single-layer structure of EVA, and its water vapor transmission rate is generally 20g / m 2 .day (38℃, 90%RH) or above. EVA is a copolymer of ethylene-vinyl acetate. Its ester bonds will hydrolyze under high temperature and high humidity conditions to produce free acetate ions, which will corrode the circuit and cause the potential induced degradation (PID) effect of photovoltaic modules.

[0004] In recent years, POE film and EVA / POE / EVA (EPE) film have been developed. POE is a copolymer of ethylene and butene or octene, a non-polar material, with a much higher volume resistivity and water vapor permeability than EVA, so it has stronger anti-PID ability. However, the price of POE particles is expensive, which makes the cost of POE film much higher than that of EVA film. Therefore, EPE film has achieved a balance between cost and performance, but because EVA and POE are different materials, the adhesion between their layers is weak, so that EPE film may have the risk of delamination. In addition, when processing the film, a variety of additives need to be added. The additives are generally polar and have better compatibility with polar EVA. Therefore, over time, the additives in the POE layer will continue to migrate to the EVA layer with strong polarity and strong absorption, causing changes in the internal structural properties of the film, and the bonding between POE and EVA layers decreases. There is even a risk of the POE layer being squeezed out and delaminated during component lamination. Summary of the invention

[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a multilayer photovoltaic module EPE encapsulation film, which adopts a reactive acid scavenger system, which can not only be better used in a humid and hot environment to achieve a better anti-PID effect, but also will not affect the transmittance, and can also improve the interface adhesion between layers.

[0006] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0007] A multilayer photovoltaic module EPE encapsulation film comprises a polyolefin layer and EVA layers distributed on both sides of the polyolefin layer; the main material of the polyolefin layer is a polyolefin material, the main resin of the EVA layer is an EVA resin, and the EVA layer further comprises 0.01-1% of an acid scavenger A and 0.1-5% of a catalyst relative to the weight of the acid scavenger A by weight; the polyolefin layer further comprises 0.01-1% of an acid scavenger B; the acid scavenger A is a carbodiimide or a carbodiimide compound; and the acid scavenger B is a silane coupling agent with an amino group.

[0008] Preferably, the polyolefin material is selected from one or a blend of two or more of HDPE, LDPE, LLDPE, ULDPE and POE.

[0009] Preferably, the acid scavenger A is selected from one or a combination of two or more of dicyclohexylcarbodiimide, diisopropylcarbodiimide, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide.

[0010] Preferably, the acid scavenger B is selected from one or a combination of two or more of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldiethoxysilane, anilinomethyltriethoxysilane and anilinomethyltrimethoxysilane.

[0011] Preferably, the catalyst is selected from one or a combination of two or more of 4-N,N-dimethylpyridine, 1-hydroxybenzotriazole, 4-pyrrolidinylpyridine, 1-hydroxy-7-azabenzotriazole, N-hydroxyphthalimide, and pentafluorophenol.

[0012] Furthermore, the polyolefin layer and the EVA layer further include a cross-linking agent, an auxiliary cross-linking agent and a silane coupling agent.

[0013] Preferably, the crosslinking agent is an organic peroxide crosslinking agent, and the organic peroxide crosslinking agent is selected from diisopropylbenzene peroxide, tert-butyl peroxy-2-ethylhexyl carbonate, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, tert-amyl peroxy-2-ethylhexyl carbonate, di(2-ethyl)hexyl peroxydicarbonate, tert-amyl peroxy-2-ethylhexyl carbonate, benzoyl peroxide, tert-butyl peroxy-2-ethylhexanoate, or a combination of two or more thereof;

[0014] The auxiliary cross-linking agent is selected from one or a combination of two or more of triallyl isocyanurate, 3-(trimethoxysilyl)propyl methacrylate, 3-vinylphenol, triallyl cyanurate, trimethylolpropane triacrylate, and trimethylolpropane trimethacrylate;

[0015] The silane coupling agent is selected from one or a combination of two or more of vinyl triethoxysilane, vinyl trimethoxysilane, vinyl triperoxide tert-butyl silane, vinyl triacetoxysilane, vinyl tri(β-methoxyethoxy)silane, and γ-(methacryloyloxy)propyl trimethoxysilane.

[0016] Furthermore, the polyolefin layer and the EVA layer further include one or more of an antioxidant, a light stabilizer, an ultraviolet absorber, and a filler.

[0017] Preferably, the antioxidant is selected from one of antioxidant 1076, antioxidant 1010, and antioxidant 168;

[0018] The light stabilizer is selected from one or more of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, poly(1-hydroxyethyl-2,2,6,6-tetramethyl-4-hydroxypiperidinyl) succinate, 2-hydroxy-4-n-octyloxybenzophenone and light stabilizer LQ-292;

[0019] The ultraviolet absorber is selected from N-(2-ethoxyphenyl)-N'-(2-ethylphenyl)-oxamide, 5-aminosalicylic acid, isooctyl salicylate, isooctyl p-methoxycinnamate, 2-hydroxy-4-n-octyloxybenzophenone, 2,2'-tetramethylenebis(3,1-benzoxazine-4-one), 2,8-dimethyl-4H,6H-benzo(1,2-d;5,4-d')bis(1,3)-oxazine-4,6-dione, 2-hydroxy-4-methoxy-2'-carboxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2-hydroxy-4-benzoyloxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone , 2-hydroxy-5-chlorobenzophenone, 2-(2'-hydroxy-5'-tert-butylphenyl)benzotriazole, 2-(2'-hydroxy-5'-aminophenyl)benzotriazole, bisphenol A disalicylate, 2-(2-hydroxy-3,5-di-tert-amylphenyl)benzotriazole, 2,2'-(1,4-phenylene)bis-4H-3,1-benzoxazine-4-one, 2-(2'-hydroxy-3',5'-dimethylphenyl)benzotriazole, 2-(2'-methyl-4'-hydroxyphenyl)benzotriazole, bis-(2-methoxy-4-hydroxy-5-benzoylphenyl)methane, 2-(2'-hydroxy-5-methylphenyl)benzotriazole, 2-(2'-hydroxy-5-methylphenyl)-5-carboxylic acid butyl ester benzotriazole one or more;

[0020] The filler is selected from one or more of titanium dioxide, calcium carbonate, barium sulfate, silicon dioxide, silicon micropowder, calcium sulfate, and bismuth oxychloride.

[0021] Furthermore, the thickness of the polyolefin layer is 50-200 μm, the thickness of the transition layer is 10-100 μm, and the thickness of the EVA layer is 30-200 μm.

[0022] The beneficial effects of the present invention are:

[0023] In the EVA layer of the present invention, carbodiimide or carbodiimide compounds are added, and a silane coupling agent with an amino group is added to the polyolefin layer. In a hot and humid environment, the carbodiimide or carbodiimide compounds in the EVA layer can react with the generated acetic acid or acidic substances to achieve the effect of deacidification; further, since the polar components in the polyolefin layer migrate to the EVA layer, the silane coupling agent with an amino group reaches the interface between the EVA layer and the polyolefin layer by utilizing the migration of the polar components, and the silane coupling agent with an amino group can react with the acetic acid or acidic substances generated by the EVA layer under the action of the carbodiimide or carbodiimide compounds, thereby improving the adhesion at the interface, avoiding the risk of decreased interlayer bonding and extrusion and delamination of the polyolefin layer. In addition, when the polar components migrate to the EVA layer, the silane coupling agent with an amino group can also enter the EVA layer, and react with acetic acid or acidic substances under the action of the carbodiimide or carbodiimide compounds, further improving the anti-PID effect.

[0024] The present invention uses two acid scavengers in synergy, and maintains the adhesion performance of the interface through the acid removal condensation reaction in a hot and humid environment, which can enhance the interface adhesion, especially the interface adhesion after hot and humid aging; and the present invention uses two acid scavengers in synergy, which can achieve better anti-PID effect;

[0025] The packaging film of the present invention adopts a reactive acid scavenger, which can not only obtain a better anti-PID effect, but also ensure that the interlayer peeling strength of the multi-layer packaging film does not decrease after long-term use, and does not affect the light transmittance. DETAILED DESCRIPTION

[0026] The technical solutions in the present invention will be described clearly and completely below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] The invention provides a multilayer photovoltaic component EPE encapsulation film, comprising a polyolefin layer and EVA layers distributed on both sides of the polyolefin layer; the main material of the polyolefin layer is a polyolefin material, the main resin of the EVA layer is an EVA resin, and the EVA layer further comprises 0.01-1% of an acid scavenger A and 0.1-5% of a catalyst relative to the weight of the acid scavenger A by weight; the polyolefin layer further comprises 0.01-1% of an acid scavenger B; the acid scavenger A is a carbodiimide or a carbodiimide compound; and the acid scavenger B is a silane coupling agent with an amino group.

[0028] Wherein, the polyolefin material is selected from one or a blend of two or more of HDPE, LDPE, LLDPE, ULDPE and POE.

[0029] The acid scavenger A is selected from one or a combination of two or more of dicyclohexylcarbodiimide, diisopropylcarbodiimide, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide.

[0030] The acid scavenger B is selected from one or a combination of two or more of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldiethoxysilane, anilinomethyltriethoxysilane and anilinomethyltrimethoxysilane.

[0031] The catalyst is selected from one or a combination of two or more of 4-N,N-dimethylpyridine, 1-hydroxybenzotriazole, 4-pyrrolidinylpyridine, 1-hydroxy-7-azabenzotriazole, N-hydroxyphthalimide and pentafluorophenol.

[0032] The polyolefin layer and the EVA layer further include a crosslinking agent, a crosslinking aid and a silane coupling agent, respectively. Specifically, in the polyolefin layer, except for the above-mentioned deacidifying agent B, the weight percentages of the polyolefin material and other components are: 95%-98.5% of the polyolefin material, 0.5-1.5% of the crosslinking agent, 0.5-1.5% of the crosslinking aid, and 0.1-1% of the silane coupling agent; in the EVA layer, except for the above-mentioned deacidifying agent A and the catalyst, the weight percentages of the EVA resin and other components are: 95%-98% of the EVA resin, 0.5-1.5% of the crosslinking agent, 0.5-1.5% of the crosslinking aid, and 0.1-1% of the silane coupling agent.

[0033] Wherein, the crosslinking agent is an organic peroxide crosslinking agent, and the organic peroxide crosslinking agent is selected from one or a combination of two or more of diisopropylbenzene peroxide, tert-butyl peroxy-2-ethylhexyl carbonate, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, tert-amyl peroxy-2-ethylhexyl carbonate, di(2-ethyl)hexyl peroxydicarbonate, tert-amyl peroxy-2-ethylhexyl carbonate, benzoyl peroxide, and tert-butyl peroxy-2-ethylhexanoate;

[0034] The auxiliary cross-linking agent is selected from one or a combination of two or more of triallyl isocyanurate, 3-(trimethoxysilyl)propyl methacrylate, 3-vinylphenol, triallyl cyanurate, trimethylolpropane triacrylate, and trimethylolpropane trimethacrylate;

[0035] The silane coupling agent is selected from one or a combination of two or more of vinyl triethoxysilane, vinyl trimethoxysilane, vinyl triperoxide tert-butyl silane, vinyl triacetoxysilane, vinyl tri(β-methoxyethoxy)silane, and γ-(methacryloyloxy)propyl trimethoxysilane.

[0036] Furthermore, the polyolefin layer and the EVA layer also include one or more of an antioxidant, a light stabilizer, an ultraviolet absorber, and a filler.

[0037] Wherein, the antioxidant is selected from one of antioxidant 1076, antioxidant 1010, and antioxidant 168;

[0038] The light stabilizer is selected from one or more of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, poly(1-hydroxyethyl-2,2,6,6-tetramethyl-4-hydroxypiperidinyl) succinate, 2-hydroxy-4-n-octyloxybenzophenone and light stabilizer LQ-292;

[0039] The ultraviolet absorber is selected from N-(2-ethoxyphenyl)-N'-(2-ethylphenyl)-oxamide, 5-aminosalicylic acid, isooctyl salicylate, isooctyl p-methoxycinnamate, 2-hydroxy-4-n-octyloxybenzophenone, 2,2'-tetramethylenebis(3,1-benzoxazine-4-one), 2,8-dimethyl-4H,6H-benzo(1,2-d;5,4-d')bis(1,3)-oxazine-4,6-dione, 2-hydroxy-4-methoxy-2'-carboxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2-hydroxy-4-benzoyloxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone , 2-hydroxy-5-chlorobenzophenone, 2-(2'-hydroxy-5'-tert-butylphenyl)benzotriazole, 2-(2'-hydroxy-5'-aminophenyl)benzotriazole, bisphenol A disalicylate, 2-(2-hydroxy-3,5-di-tert-amylphenyl)benzotriazole, 2,2'-(1,4-phenylene)bis-4H-3,1-benzoxazine-4-one, 2-(2'-hydroxy-3',5'-dimethylphenyl)benzotriazole, 2-(2'-methyl-4'-hydroxyphenyl)benzotriazole, bis-(2-methoxy-4-hydroxy-5-benzoylphenyl)methane, 2-(2'-hydroxy-5-methylphenyl)benzotriazole, 2-(2'-hydroxy-5-methylphenyl)-5-carboxylic acid butyl ester benzotriazole one or more;

[0040] The filler is selected from one or more of titanium dioxide, calcium carbonate, barium sulfate, silicon dioxide, silicon micropowder, calcium sulfate, and bismuth oxychloride.

[0041] The thickness of the polyolefin layer is 50-200 μm, and the thickness of the EVA layer is 30-200 μm.

[0042] Example 1

[0043] Based on 100 parts by total weight, the raw materials for preparing the polyolefin layer include:

[0044] 97.2 parts of POE resin, 1 part of acid scavenger B: γ-aminopropyltrimethoxysilane, 0.3 parts of cross-linking agent peroxy-2-ethylhexyl carbonate tert-butyl ester, 0.3 parts of peroxy-2-ethylhexyl carbonate tert-amyl ester, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 292.

[0045] Based on 100 parts by total weight, the raw materials for preparing the EVA layer include:

[0046] 97.15 parts of EVA resin, 1 part of acid scavenger A: dicyclohexylcarbodiimide, 0.05 parts of catalyst 4-N,N-dimethylpyridine, 0.3 parts of cross-linking agent tert-butyl peroxide-2-ethylhexyl carbonate, 0.3 parts of tert-amyl peroxide 2-ethylhexyl carbonate, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 770.

[0047] The raw materials used for the preparation of the polyolefin layer and the EVA layer are stirred separately, placed at 35°C for 12 hours, and then put into a multi-layer co-extrusion process equipment. The extruder speed or melt pump speed is adjusted according to the thickness, and 3 layers of film material are extruded. After cooling and shaping, the required multi-layer photovoltaic module EPE encapsulation film can be obtained. The thickness of the polyolefin layer is 120μm, and the thickness of the two EVA layers is 150μm.

[0048] Example 2

[0049] Based on 100 parts by total weight, the raw materials for preparing the polyolefin layer include:

[0050] 97.2 parts of POE resin, 1 part of acid scavenger B: γ-aminopropyltrimethoxysilane, 0.3 parts of cross-linking agent peroxy-2-ethylhexyl carbonate tert-butyl ester, 0.3 parts of peroxy-2-ethylhexyl carbonate tert-amyl ester, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 292.

[0051] Based on 100 parts by total weight, the raw materials for preparing the EVA layer include:

[0052] 97.67 parts of EVA resin, 0.5 parts of acid scavenger A: dicyclohexylcarbodiimide, 0.03 parts of catalyst 4-N,N-dimethylpyridine, 0.3 parts of cross-linking agent tert-butyl peroxide-2-ethylhexyl carbonate, 0.3 parts of tert-amyl peroxide 2-ethylhexyl carbonate, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 770.

[0053] The raw materials used for the preparation of the polyolefin layer and the EVA layer are stirred separately, placed at 35°C for 12 hours, and then put into a multi-layer co-extrusion process equipment. The extruder speed or melt pump speed is adjusted according to the thickness, and 3 layers of film material are extruded. After cooling and shaping, the required multi-layer photovoltaic module EPE encapsulation film can be obtained. The thickness of the polyolefin layer is 120μm, and the thickness of the two EVA layers is 150μm.

[0054] Example 3

[0055] Based on 100 parts by total weight, the raw materials for preparing the polyolefin layer include:

[0056] 98.1 parts of POE resin, 0.1 parts of acid scavenger B: γ-aminopropyltrimethoxysilane, 0.3 parts of cross-linking agent tert-butyl peroxide-2-ethylhexyl carbonate, 0.3 parts of tert-amyl peroxide 2-ethylhexyl carbonate, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 292.

[0057] Based on 100 parts by total weight, the raw materials for preparing the EVA layer include:

[0058] 97.67 parts of EVA resin, 0.5 parts of acid scavenger A: dicyclohexylcarbodiimide, 0.03 parts of catalyst 4-N,N-dimethylpyridine, 0.3 parts of cross-linking agent tert-butyl peroxide-2-ethylhexyl carbonate, 0.3 parts of tert-amyl peroxide 2-ethylhexyl carbonate, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 770.

[0059] The raw materials used for the preparation of the polyolefin layer and the EVA layer are stirred separately, placed at 35°C for 12 hours, and then put into a multi-layer co-extrusion process equipment. The extruder speed or melt pump speed is adjusted according to the thickness, and 3 layers of film material are extruded. After cooling and shaping, the required multi-layer photovoltaic module EPE encapsulation film can be obtained. The thickness of the polyolefin layer is 120μm, and the thickness of the two EVA layers is 150μm.

[0060] Comparative Example 1

[0061] Based on 100 parts by total weight, the raw materials for preparing the polyolefin layer include:

[0062] 98.2 parts of POE resin, 0.3 parts of cross-linking agent peroxy-2-ethylhexyl tert-butyl carbonate, 0.3 parts of peroxy-2-ethylhexyl tert-amyl carbonate, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 292.

[0063] Based on 100 parts by total weight, the raw materials for preparing the EVA layer include:

[0064] 98.2 parts of EVA resin, 0.3 parts of cross-linking agent peroxy-2-ethylhexyl tert-butyl carbonate, 0.3 parts of peroxy-2-ethylhexyl tert-amyl carbonate, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 770.

[0065] The raw materials used for the preparation of the polyolefin layer and the EVA layer are stirred separately, placed at 35°C for 12 hours, and then put into a multi-layer co-extrusion process equipment. The extruder speed or melt pump speed is adjusted according to the thickness, and 3 layers of film material are extruded. After cooling and shaping, the required multi-layer photovoltaic module EPE encapsulation film can be obtained. The thickness of the polyolefin layer is 120μm, and the thickness of the two EVA layers is 150μm.

[0066] Comparative Example 2

[0067] Based on 100 parts by total weight, the raw materials for preparing the polyolefin layer include:

[0068] 98.2 parts of POE resin, 0.3 parts of cross-linking agent peroxy-2-ethylhexyl tert-butyl carbonate, 0.3 parts of peroxy-2-ethylhexyl tert-amyl carbonate, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 292.

[0069] Based on 100 parts by total weight, the raw materials for preparing the EVA layer include:

[0070] 97.2 parts of EVA resin, 1.0 part of magnesium hydroxide with an average particle size of 0.5 μm, 0.3 parts of cross-linking agent tert-butyl peroxide-2-ethylhexyl carbonate, 0.3 parts of tert-amyl peroxide 2-ethylhexyl carbonate, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 770.

[0071] The raw materials used for the preparation of the polyolefin layer and the EVA layer are stirred separately, placed at 35°C for 12 hours, and then put into a multi-layer co-extrusion process equipment. The extruder speed or melt pump speed is adjusted according to the thickness, and 3 layers of film material are extruded. After cooling and shaping, the required multi-layer photovoltaic module EPE encapsulation film can be obtained. The thickness of the polyolefin layer is 120μm, and the thickness of the two EVA layers is 150μm.

[0072] Comparative Example 3

[0073] Based on 100 parts by total weight, the raw materials for preparing the polyolefin layer include:

[0074] 98.1 parts of POE resin, 0.1 parts of acid scavenger B: γ-aminopropyltrimethoxysilane, 0.3 parts of cross-linking agent tert-butyl peroxide-2-ethylhexyl carbonate, 0.3 parts of tert-amyl peroxide 2-ethylhexyl carbonate, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 292.

[0075] Based on 100 parts by total weight, the raw materials for preparing the EVA layer include:

[0076] 98.17 parts of EVA resin, 0.03 parts of catalyst 4-N,N-dimethylpyridine, 0.3 parts of cross-linking agent tert-butyl peroxide-2-ethylhexyl carbonate, 0.3 parts of tert-amyl peroxide 2-ethylhexyl carbonate, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 770.

[0077] The raw materials used for the preparation of the polyolefin layer and the EVA layer are stirred separately, placed at 35°C for 12 hours, and then put into a multi-layer co-extrusion process equipment. The extruder speed or melt pump speed is adjusted according to the thickness, and 3 layers of film material are extruded. After cooling and shaping, the required multi-layer photovoltaic module EPE encapsulation film can be obtained. The thickness of the polyolefin layer is 120μm, and the thickness of the two EVA layers is 150μm.

[0078] Comparative Example 4

[0079] Based on 100 parts by total weight, the raw materials for preparing the polyolefin layer include:

[0080] 98.2 parts of POE resin, 0.3 parts of cross-linking agent peroxy-2-ethylhexyl tert-butyl carbonate, 0.3 parts of peroxy-2-ethylhexyl tert-amyl carbonate, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 292.

[0081] Based on 100 parts by total weight, the raw materials for preparing the EVA layer include:

[0082] 97.67 parts of EVA resin, 0.5 parts of acid scavenger A: dicyclohexylcarbodiimide, 0.03 parts of catalyst 4-N,N-dimethylpyridine, 0.3 parts of cross-linking agent tert-butyl peroxide-2-ethylhexyl carbonate, 0.3 parts of tert-amyl peroxide 2-ethylhexyl carbonate, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 770.

[0083] The raw materials used for the preparation of the polyolefin layer and the EVA layer are stirred separately, placed at 35°C for 12 hours, and then put into a multi-layer co-extrusion process equipment. The extruder speed or melt pump speed is adjusted according to the thickness, and 3 layers of film material are extruded. After cooling and shaping, the required multi-layer photovoltaic module EPE encapsulation film can be obtained. The thickness of the polyolefin layer is 120μm, and the thickness of the two EVA layers is 150μm.

[0084] The light transmittance test of the packaging film samples of Examples 1-3 and Comparative Examples 1-4 was performed with reference to IEC62788-1-2.

[0085] The encapsulation film samples of Examples 1-3 and Comparative Examples 1-4 were prepared into photovoltaic modules, and the module power was tested, and the power attenuation of the module after PID192h and PID384h was tested.

[0086] To test the interlayer adhesion, the EVA layer and the POE layer can be extruded separately and laminated according to the backsheet / EVA layer / POE layer / EVA layer / backsheet, and the interlayer peel strength between the EVA layer and the POE layer and the interlayer peel strength after PCT48h and DH2000h can be tested.

[0087] The test results are shown in Table 1.

[0088]

[0089]

[0090] From the data in Table 1, we can see that:

[0091] The light transmittance of Examples 1-3 is almost unchanged compared with that of Comparative Example 1 without adding an acid scavenger, indicating that the acid scavenger of the present invention does not affect the light transmittance at a certain ratio. After adding magnesium hydroxide acid scavenger to Comparative Example 2, the light transmittance is significantly reduced.

[0092] Interlayer peel strength comparison data, initial value is not much different.After PCT48h and DH2000, Comparative Example 1 has been significantly reduced, indicating that without adding the acid scavenger system of the present invention, after PCT and DH aging, the interlayer peel strength decreases. Comparative Example 2 also significantly reduces the peel strength after PCT48h and DH2000. And embodiment 1-3, after PCT48h and DH2000, the peel strength can still keep more than 70N / cm, this is because the acid scavenger of the present invention is a reactive acid scavenger, in a hot and humid environment, by the acid removal condensation reaction, the adhesion performance of the interface is maintained. Comparative Examples 3 and 4 only add acid scavenger B or acid scavenger A respectively, and after PCT48h and DH2000, the peel strength significantly reduces, indicating that the synergy of two kinds of acid scavengers can be realized to enhance the interfacial adhesion.

[0093] Comparing PID power attenuation, PID192h and PID384h of Examples 1-3 are all within 1.5%, which have obvious anti-PID attenuation effect. Comparative Example 1 does not add acid scavenger, and its power attenuation after PID192h and PID384h can reach 3.12% and 4.52% respectively. Comparative Example 2 adds magnesium hydroxide acid scavenger to have a certain anti-PID effect, but the result is not as good as the embodiment of the present invention. Comparative Examples 3 and 4 only add acid scavenger B or acid scavenger A, and the anti-PID attenuation ability is reduced, and the attenuation after PID is larger. It shows that the two acid scavengers of the present invention can cooperate to achieve better anti-PID effect.

[0094] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0095] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A multilayer photovoltaic module EPE encapsulation film, characterized in that: The invention comprises a polyolefin layer and EVA layers distributed on both sides of the polyolefin layer; the main material of the polyolefin layer is a polyolefin material, the main resin of the EVA layer is an EVA resin, and the EVA layer further comprises 0.01-1% of an acid scavenger A and 0.1-5% of a catalyst relative to the weight of the acid scavenger A by weight; the polyolefin layer further comprises 0.01-1% of an acid scavenger B; the acid scavenger A is a carbodiimide or a carbodiimide compound; and the acid scavenger B is a silane coupling agent with an amino group.

2. A multilayer photovoltaic module EPE encapsulation film according to claim 1, characterized in that: The polyolefin material is selected from one or a blend of two or more of HDPE, LDPE, LLDPE, ULDPE and POE.

3. A multilayer photovoltaic module EPE encapsulation film according to claim 1, characterized in that: The acid scavenger A is selected from one or a combination of two or more of dicyclohexylcarbodiimide, diisopropylcarbodiimide, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide.

4. A multilayer photovoltaic module EPE encapsulation film according to claim 1, characterized in that: The acid scavenger B is selected from one or a combination of two or more of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldiethoxysilane, anilinomethyltriethoxysilane and anilinomethyltrimethoxysilane.

5. A multi-layer photovoltaic module EPE encapsulation film according to claim 1, characterized in that: The catalyst is selected from one or a combination of two or more of 4-N,N-dimethylpyridine, 1-hydroxybenzotriazole, 4-pyrrolidinylpyridine, 1-hydroxy-7-azabenzotriazole, N-hydroxyphthalimide and pentafluorophenol.

6. A multilayer photovoltaic module EPE encapsulation film according to claim 1, characterized in that: The polyolefin layer and the EVA layer further include a cross-linking agent, an auxiliary cross-linking agent and a silane coupling agent respectively.

7. A multi-layer photovoltaic module EPE encapsulation film according to claim 6, characterized in that: The crosslinking agent is an organic peroxide crosslinking agent, and the organic peroxide crosslinking agent is selected from one or a combination of two or more of diisopropylbenzene peroxide, tert-butyl peroxy-2-ethylhexyl carbonate, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, tert-amyl peroxy-2-ethylhexyl carbonate, di(2-ethyl)hexyl peroxydicarbonate, tert-amyl peroxy-2-ethylhexyl carbonate, benzoyl peroxide, and tert-butyl peroxy-2-ethylhexanoate; The auxiliary cross-linking agent is selected from one or a combination of two or more of triallyl isocyanurate, 3-(trimethoxysilyl)propyl methacrylate, 3-vinylphenol, triallyl cyanurate, trimethylolpropane triacrylate, and trimethylolpropane trimethacrylate; The silane coupling agent is selected from one or a combination of two or more of vinyl triethoxysilane, vinyl trimethoxysilane, vinyl triperoxide tert-butyl silane, vinyl triacetoxysilane, vinyl tri(β-methoxyethoxy)silane, and γ-(methacryloyloxy)propyl trimethoxysilane.

8. A multi-layer photovoltaic module EPE encapsulation film according to claim 1 or 6, characterized in that: The polyolefin layer and the EVA layer further include one or more of an antioxidant, a light stabilizer, an ultraviolet absorber, and a filler.

9. A multi-layer photovoltaic module EPE encapsulation film according to claim 8, characterized in that: The antioxidant is selected from one of antioxidant 1076, antioxidant 1010, and antioxidant 168; The light stabilizer is selected from one or more of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, poly(1-hydroxyethyl-2,2,6,6-tetramethyl-4-hydroxypiperidinyl) succinate, 2-hydroxy-4-n-octyloxybenzophenone and light stabilizer LQ-292; The ultraviolet absorber is selected from N-(2-ethoxyphenyl)-N'-(2-ethylphenyl)-oxamide, 5-aminosalicylic acid, isooctyl salicylate, isooctyl p-methoxycinnamate, 2-hydroxy-4-n-octyloxybenzophenone, 2,2'-tetramethylenebis(3,1-benzoxazine-4-one), 2,8-dimethyl-4H,6H-benzo(1,2-d;5,4-d')bis(1,3)-oxazine-4,6-dione, 2-hydroxy-4-methoxy-2'-carboxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2-hydroxy-4-benzoyloxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone , 2-hydroxy-5-chlorobenzophenone, 2-(2'-hydroxy-5'-tert-butylphenyl)benzotriazole, 2-(2'-hydroxy-5'-aminophenyl)benzotriazole, bisphenol A disalicylate, 2-(2-hydroxy-3,5-di-tert-amylphenyl)benzotriazole, 2,2'-(1,4-phenylene)bis-4H-3,1-benzoxazine-4-one, 2-(2'-hydroxy-3',5'-dimethylphenyl)benzotriazole, 2-(2'-methyl-4'-hydroxyphenyl)benzotriazole, bis-(2-methoxy-4-hydroxy-5-benzoylphenyl)methane, 2-(2'-hydroxy-5-methylphenyl)benzotriazole, 2-(2'-hydroxy-5-methylphenyl)-5-carboxylic acid butyl ester benzotriazole one or more; The filler is selected from one or more of titanium dioxide, calcium carbonate, barium sulfate, silicon dioxide, silicon micropowder, calcium sulfate, and bismuth oxychloride.

10. The multi-layer photovoltaic module EPE encapsulation film according to claim 1, characterized in that: The thickness of the polyolefin layer is 50-200 μm, and the thickness of the EVA layer is 30-200 μm.

Citation Information

Cited By

  • Composite membrane as well as preparation method and application thereof

    CN120327048A