PU reflective hot paste and manufacturing method thereof

By using multi-performance rubber and anti-aging additives in PU reflective thermal paste to enhance the performance of the adhesive, the aging resistance and corrosion resistance of the reflective thermal paste is solved, and the bonding strength and service life are significantly improved.

CN118909558APending Publication Date: 2024-11-08ZHEJIANG HAICHUAN SECURITY SUPPLIES CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410955766.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

PU reflective thermal thread has general aging resistance and corrosion resistance, high temperature resistance and insufficient bonding strength, easy to fall off, and short service life.

Method used

Multi-performance rubber and anti-aging additives are used to participate in the preparation of composite adhesives. The modification reaction enhances the cohesion, high temperature and corrosion resistance of the adhesive, and is used in reflective thermal pastes to improve bonding strength and anti-aging. performance.

Benefits of technology

It effectively enhances the bonding strength of reflective thermal patches, high temperature resistance and ultraviolet and thermal oxygen aging properties, making it difficult to fall off in high temperature and corrosive environments, extending service life and expanding the field of use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909558A_ABST
    Figure CN118909558A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of reflective hot stickers, and discloses a PU reflective hot sticker and a manufacturing method thereof.The PU reflective hot sticker comprises a reflective layer, a polypropylene base film layer, a binder layer and a release film layer from top to bottom, and the reflective layer is obtained by coating one side of a polypropylene base film with a composite binder, evenly laying glass beads and conducting extrusion and compaction through a hot roller; the adhesive layer is formed by uniformly coating the other side of the polypropylene base film with a composite adhesive and curing the composite adhesive, the multi-performance rubber and the anti-aging additive are prepared to participate in the preparation process of the composite adhesive, the bonding strength of the reflective hot paste can be effectively enhanced, and the reflective hot paste is resistant to high temperature, ultraviolet and thermo-oxidative aging and can be applied to the field of reflective hot paste. The paint can be used for a long time in an environment with a corrosive medium, and has a wide application field and a long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of reflective heat stickers, and in particular to a PU reflective heat sticker and a manufacturing method thereof. Background Art

[0002] Reflective heat transfer stickers are also called reflective heat transfer films. They are usually transferred using a heat press at appropriate pressure and temperature. Through the retro-reflection phenomenon, they produce excellent reflective effects. At night or in environments with poor visibility, they can significantly improve the visibility of objects and serve as a safety warning. They have been widely used in road traffic safety, occupational safety, and artistic creation and decoration. Among the many reflective heat transfer stickers, PU reflective heat transfer stickers use polyurethane materials as the base material, have excellent weather resistance and elasticity, and can be used in a variety of occasions that require reflective effects. They are used frequently and have good reflective effects. They are currently one of the most commonly used reflective heat transfer stickers.

[0003] However, ordinary PU reflective thermal stickers have average high temperature resistance and corrosion resistance in actual use, and their UV resistance and thermal oxidation aging resistance are not strong. When used in corresponding scenarios, the bonding strength will be reduced, and it is very likely to fall off and warp, which seriously limits the use of PU reflective thermal stickers. Therefore, people often make improvements to them when using PU reflective thermal stickers. For example, the patent with publication number CN114921201B discloses an adhesive composition for high-brightness reflective thermal stickers and a preparation method thereof. The composite adhesive component of specific specifications is used to achieve an effective combination of reflective clothing substrate and reflective particles, and improve the adhesion of the adhesive composition on the surface of the thermal sticker. At the same time, it has flexibility and folding resistance, good compatibility between the components, strong temperature resistance, and broad application prospects. The patent improves the adhesive of the reflective thermal sticker. Although the bonding performance is enhanced, no improvement is made in the anti-aging performance. In a long-term sunlight environment and a hot and humid environment, the aging process of the reflective thermal sticker is accelerated, affecting the service life. Summary of the invention

[0004] The purpose of the present invention is to provide a reflective heat patch and a manufacturing method thereof, which solves the following problems: PU reflective heat patch has average aging resistance and corrosion resistance, insufficient high temperature resistance and bonding strength, is easy to fall off, and has a short service life.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for making a PU reflective heat patch comprises the following steps:

[0007] (1) The composite adhesive is evenly coated on one side of the polypropylene base film, glass beads are evenly laid, and a hot roller is used for extrusion and compaction at 100-120° C. to obtain a reflective layer;

[0008] (2) evenly coating the composite adhesive on the other side of the polypropylene base film, curing at 80-90° C. for 15-20 min to form an adhesive layer, and covering with a silicone release film to obtain a PU reflective heat transfer sticker;

[0009] The coating thickness of the composite adhesive in the reflective layer is 20-25 μm; the coating thickness of the composite adhesive in the adhesive layer is 25-55 μm;

[0010] The composite adhesive comprises the following raw materials in parts by weight: 20-30 parts of isophorone diisocyanate, 15-20 parts of polytetramethylene ether glycol, 10-12 parts of multi-performance rubber, 1-2 parts of dibutyltin dilaurate, 3-5 parts of 1,4-butanediol, 5-8 parts of anti-aging additives, 3-6 parts of triethylamine, 30-50 parts of deionized water, 2-3 parts of plasticizer, and 1-3 parts of defoaming agent.

[0011] Furthermore, the plasticizer is diisononyl phthalate or diisooctyl phthalate; and the defoaming agent is dimethyl silicone oil or polyethylene glycol.

[0012] Furthermore, the preparation method of the multi-performance rubber comprises the following steps:

[0013] S1: Put EPDM rubber in toluene, introduce nitrogen, add 4-maleimidobutyric acid and initiator, heat to 60-70°C and stir for 8-10h, collect the product after reduced pressure distillation, and obtain modified rubber;

[0014] S2: Place the modified rubber and glycidyl furfuryl ether in N,N-dimethylformamide, mix thoroughly, add the catalyst, heat to 55-65°C and react for 6-8h, remove the solvent by rotary evaporation and collect the product to obtain a multi-performance rubber.

[0015] In this scheme, under the action of an initiator, the active double bonds in the EPDM rubber structure undergo free radical polymerization reaction with the double bonds in the 4-maleimidebutyric acid structure to obtain a modified rubber having a carboxyl group and a maleimide group in the structure. Then, under the action of a catalyst, the carboxyl group in the modified rubber structure undergoes a ring-opening reaction with the epoxy group in the glycidyl furfuryl ether structure to obtain a multi-performance rubber having multiple hydroxyl groups. The hydroxyl groups in the multi-performance rubber structure can participate in the preparation process of the composite adhesive, enhance the cohesion of the composite adhesive, and enhance its bonding strength. At the same time, the maleimide group and furan group in the multi-performance rubber structure can enhance the high temperature resistance and corrosion resistance of the composite adhesive, thereby ensuring that the reflective heat patch prepared using the composite adhesive is not easy to fall off when used in an environment with high temperature or corrosive media, effectively enhancing the use field of the reflective heat patch and giving it a long service life.

[0016] Furthermore, in step S1, the initiator is benzoyl peroxide or dicumyl peroxide.

[0017] Furthermore, in step S2, the catalyst is any one of tetrabutylammonium bromide, tetrabutylammonium hydrogen sulfate, and tetrabutylammonium hydroxide.

[0018] Furthermore, the preparation method of the anti-aging additive comprises the following steps:

[0019] SS1: Place nano zinc oxide in tetrahydrofuran, ultrasonically disperse for 15-20 minutes, add trimellitic anhydride formyl chloride and pyridine, place in an ice-water bath, let stand, filter, wash and dry to obtain modified nano zinc oxide;

[0020] SS2: Place the modified nano zinc oxide in xylene, ultrasonically disperse for 10-15 minutes, add 3,5-di-tert-butyl-4-hydroxybenzyl alcohol and p-toluenesulfonic acid, heat to 55-70°C and react for 6-8 hours, filter, wash, dry and collect the product to obtain an anti-aging additive.

[0021] In this scheme, under the action of pyridine, the hydroxyl groups on the surface of nano zinc oxide react with the acyl chloride groups in the structure of trimellitic anhydride formyl chloride to obtain modified nano zinc oxide with an anhydride structure, and then under the action of p-toluenesulfonic acid, the anhydride groups on the surface of the modified nano zinc oxide react with the hydroxyl groups in the structure of 3,5-di-tert-butyl-4-hydroxybenzyl alcohol to obtain an anti-aging additive. The anti-aging additive has excellent anti-ultraviolet aging ability based on nano zinc oxide, and its surface is coated with hindered phenol groups, which has excellent antioxidant ability. The multiple carboxyl groups on its surface can also participate in the preparation process of the composite adhesive, so that the prepared composite adhesive has excellent anti-ultraviolet aging and thermal oxygen aging ability, and can effectively prevent the problem of accelerated aging process caused by long-term use of the reflective heat transfer sticker exposed to sunlight and thermal oxygen environment, effectively solve the problem of shedding of the reflective heat transfer sticker due to aging, and significantly enhance the service life of the reflective heat transfer sticker.

[0022] Furthermore, in step SS1, the temperature of the ice water bath is 4-6°C and the time is 3-5h.

[0023] Furthermore, the preparation method of the composite binder comprises the following steps:

[0024] Step 1: Mix isophorone diisocyanate, polytetramethylene glycol, and multi-performance rubber, introduce nitrogen, add dibutyltin dilaurate, stir evenly, heat to 60-65° C. and react for 3-5 hours, and collect the product to obtain a polyurethane prepolymer;

[0025] Step 2: Add 1,4-butanediol and anti-aging additives to the polyurethane prepolymer, continue to react for 2-3 hours, cool to 35-40°C, add triethylamine to neutralize for 10-15 minutes, add deionized water, stir for 1-2 hours, add plasticizer and defoamer, stir well, and let stand to defoam, to obtain a composite adhesive.

[0026] A PU reflective heat patch is prepared by the preparation method described in any one of claims 1 to 8.

[0027] Beneficial effects of the present invention:

[0028] The present invention prepares multi-performance rubber and anti-aging additives in the preparation process of the composite adhesive, and applies them to the reflective heat patch, which can effectively enhance the bonding strength of the reflective heat patch, and has high temperature resistance, UV resistance and thermal oxygen aging resistance. It can be used for a long time in an environment with corrosive media, has a wide range of uses and a long service life.

[0029] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0031] Figure 1 This is a thermal weight loss curve of nano zinc oxide, modified nano zinc oxide, and anti-aging additives in the embodiments of the present invention. DETAILED DESCRIPTION

[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] The preparation methods of the multi-performance rubber and the anti-aging additives in the following embodiments and comparative examples of the present invention are as follows:

[0034] 1. Preparation of multi-performance rubber

[0035] S1: 3 g of EPDM rubber was placed in 60 ml of toluene, nitrogen was introduced, 2.8 g of 4-maleimidobutyric acid and 0.2 g of benzoyl peroxide were added, the temperature was raised to 60 °C and stirred for 8 h, and the product was collected after reduced pressure distillation to obtain a modified rubber;

[0036] The acid-base titration method is used to test the carboxyl content in the modified rubber. The specific operation is as follows: 1g of the modified rubber is placed as a sample in a 50ml acetone solution, an excess of a potassium hydroxide ethanol standard solution with a concentration of 1mol / L is added, 2 drops of phenolphthalein indicator are added, and after sufficient mixing, a back titration is performed using a hydrochloric acid standard solution with a concentration of 1mol / L. After the color changes significantly, the titration is stopped, and a blank experiment is performed at the same time. The volume of the potassium hydroxide ethanol standard solution and the volume of the hydrochloric acid standard solution consumed are recorded and calculated according to the following formula: W=45×c(V-V0)×100% / M; wherein W is the mass fraction of the carboxyl group in the modified rubber, %; c is the concentration of the hydrochloric acid standard solution, mol / L; V is the volume of the hydrochloric acid standard solution consumed, ml; V0 is the volume of the hydrochloric acid standard solution consumed in the blank sample, ml; M is the sample mass, g; 45 is the molar mass of the carboxyl group, g / mol; after calculation, the carboxyl content in the modified rubber is 6.3%.

[0037] S2: 3.5 g of modified rubber and 3.2 g of glycidyl furfuryl ether were placed in 100 ml of N,N-dimethylformamide, and after thorough mixing, 0.03 g of tetrabutylammonium bromide was added, and the temperature was raised to 55°C for reaction for 6 h. After rotary evaporation to remove the solvent, the product was collected to obtain a multi-performance rubber.

[0038] The carboxyl content in the multi-performance rubber was tested by acid-base titration. The specific operation steps were the same as S1. After calculation, the carboxyl content in the multi-performance rubber was 1.3%. The decrease in the carboxyl content was due to the ring-opening reaction between the carboxyl in the modified rubber and the epoxy group in the glycidyl furfural structure, which consumed the carboxyl.

[0039] A free radical polymerization reaction is generated between the double bonds in the structure of EPDM rubber and the double bonds in the structure of 4-maleimidobutyric acid, thereby introducing a maleimide structure into the structure of EPDM rubber. A ring-opening reaction is then generated between the carboxyl group in the modified rubber structure and the epoxy group in the glycidyl furfuryl ether structure, thereby introducing an ether bond and a furan group into the modified rubber structure to obtain a multi-performance rubber.

[0040] 2. Preparation of anti-aging additives

[0041] SS1: 2.6 g of nano zinc oxide was placed in 120 ml of tetrahydrofuran, and ultrasonically dispersed for 15 min. Then, 2 g of trimellitic anhydride formoyl chloride and 0.05 g of pyridine were added. The mixture was placed in an ice-water bath at 4 °C for 3 h. After standing, the mixture was filtered, washed, and dried to obtain modified nano zinc oxide.

[0042] SS2: Place 3g of modified nano zinc oxide in 150ml of xylene, ultrasonically disperse for 10min, add 3.2g of 3,5-di-tert-butyl-4-hydroxybenzyl alcohol and 0.05g of p-toluenesulfonic acid, heat to 55°C and react for 6h, collect the product after filtering, washing and drying to obtain the anti-aging additive.

[0043] Nano zinc oxide, modified nano zinc oxide and anti-aging filler were analyzed by thermogravimetric analysis. Figure 1 It can be seen that the final mass retention rate of nano zinc oxide at high temperature is 97.4%; the final mass retention rate of modified nano zinc oxide at high temperature is 56.2%; the final mass retention rate of anti-aging additives is 27.3%; the part of nano zinc oxide lost at high temperature is caused by the thermal decomposition of crystalline water in its structure, the part of modified nano zinc oxide lost at high temperature is caused by the thermal decomposition of trimellitic anhydride formyl chloride grafted on its surface, and the part of anti-aging additives lost at high temperature is caused by the thermal decomposition of organic matter grafted on its surface.

[0044] The surface of nano zinc oxide is modified by trimellitic anhydride formyl chloride, anhydride groups are introduced on the surface, and then the hydroxyl groups in the structure of 3,5-di-tert-butyl-4-hydroxybenzyl alcohol undergo a ring-opening reaction with the anhydride groups on its surface to obtain an anti-aging additive with carboxyl groups and hindered phenol groups on the surface.

[0045] Example 1

[0046] Preparation of composite adhesive

[0047] Step 1: 20 g of isophorone diisocyanate, 15 g of polytetramethylene ether glycol, and 10 g of multi-performance rubber are mixed, nitrogen is introduced, 1 g of dibutyltin dilaurate is added, the mixture is stirred evenly, the temperature is raised to 60° C. for reaction for 3 h, and the product is collected to obtain a polyurethane prepolymer;

[0048] Step 2: Add 3 g of 1,4-butanediol and 5 g of anti-aging additive to the polyurethane prepolymer, continue the reaction for 2 h, cool to 35 ° C, add 3 g of triethylamine to neutralize for 10 min, add 30 ml of deionized water, stir for 1 h, add 2 g of diisononyl phthalate and 1 g of dimethyl silicone oil, stir well, and let stand to defoam to obtain a composite adhesive.

[0049] Example 2

[0050] Preparation of composite adhesive

[0051] Step 1: 25 g of isophorone diisocyanate, 18 g of polytetramethylene ether glycol, and 11 g of multi-performance rubber were mixed, nitrogen was introduced, 1.5 g of dibutyltin dilaurate was added, the mixture was stirred evenly, the temperature was raised to 62° C. and the mixture was reacted for 4 h, and the product was collected to obtain a polyurethane prepolymer;

[0052] Step 2: Add 4 g of 1,4-butanediol and 7 g of anti-aging additive to the polyurethane prepolymer, continue the reaction for 2.5 h, cool to 38 ° C, add 4.5 g of triethylamine to neutralize for 12 min, add 40 ml of deionized water, stir for 1.5 h, add 2.5 g of diisooctyl phthalate and 1.5 g of dimethyl silicone oil, stir well, and let stand to defoam to obtain a composite adhesive.

[0053] Example 3

[0054] Preparation of composite adhesive

[0055] Step 1: 30 g of isophorone diisocyanate, 20 g of polytetramethylene ether glycol, and 12 g of multi-performance rubber are mixed, nitrogen is introduced, 2 g of dibutyltin dilaurate is added, the mixture is stirred evenly, the temperature is raised to 60° C. and the mixture is reacted for 3 h, and the product is collected to obtain a polyurethane prepolymer;

[0056] Step 2: Add 5 g of 1,4-butanediol and 8 g of anti-aging additive to the polyurethane prepolymer, continue the reaction for 3 h, cool to 40 ° C, add 6 g of triethylamine to neutralize for 15 min, add 50 ml of deionized water, stir for 2 h, add 3 g of diisononyl phthalate and 3 g of polyethylene glycol, stir well, and let stand to defoam to obtain a composite adhesive.

[0057] Comparative Example 1

[0058] Preparation of composite adhesive

[0059] Step 1: 25 g of isophorone diisocyanate and 18 g of polytetramethylene glycol were mixed, nitrogen was introduced, 1.5 g of dibutyltin dilaurate was added, the mixture was stirred evenly, the temperature was raised to 62° C. and the mixture was reacted for 4 h, and the product was collected to obtain a polyurethane prepolymer;

[0060] Step 2: Add 4 g of 1,4-butanediol and 7 g of anti-aging additive to the polyurethane prepolymer, continue the reaction for 2.5 h, cool to 38 ° C, add 4.5 g of triethylamine to neutralize for 12 min, add 40 ml of deionized water, stir for 1.5 h, add 2.5 g of diisooctyl phthalate and 1.5 g of dimethyl silicone oil, stir well, and let stand to defoam to obtain a composite adhesive.

[0061] Comparative Example 2

[0062] Preparation of composite adhesive

[0063] Step 1: 25 g of isophorone diisocyanate, 18 g of polytetramethylene ether glycol, and 11 g of multi-performance rubber were mixed, nitrogen was introduced, 1.5 g of dibutyltin dilaurate was added, the mixture was stirred evenly, the temperature was raised to 62° C. and the mixture was reacted for 4 h, and the product was collected to obtain a polyurethane prepolymer;

[0064] Step 2: Add 4 g of 1,4-butanediol to the polyurethane prepolymer, continue the reaction for 2.5 h, cool to 38 ° C, add 4.5 g of triethylamine to neutralize for 12 min, add 40 ml of deionized water, stir for 1.5 h, add 2.5 g of diisooctyl phthalate and 1.5 g of dimethyl silicone oil, stir well, and let stand to defoam to obtain a composite adhesive.

[0065] Comparative Example 3

[0066] Preparation of composite adhesive

[0067] Step 1: 25 g of isophorone diisocyanate and 18 g of polytetramethylene glycol were introduced with nitrogen, 1.5 g of dibutyltin dilaurate was added, the mixture was stirred evenly, the temperature was raised to 62° C. and the mixture was reacted for 4 h, and the product was collected to obtain a polyurethane prepolymer;

[0068] Step 2: Add 4 g of 1,4-butanediol to the polyurethane prepolymer, continue the reaction for 2.5 h, cool to 38 ° C, add 4.5 g of triethylamine to neutralize for 12 min, add 40 ml of deionized water, stir for 1.5 h, add 2.5 g of diisooctyl phthalate and 1.5 g of dimethyl silicone oil, stir well, and let stand to defoam to obtain a composite adhesive.

[0069] Comparative Example 4

[0070] Preparation of composite adhesive

[0071] Step 1: 25 g of isophorone diisocyanate, 18 g of polytetramethylene ether glycol, and 11 g of modified rubber were mixed, nitrogen was introduced, 1.5 g of dibutyltin dilaurate was added, the mixture was stirred evenly, the temperature was raised to 62° C. and the mixture was reacted for 4 h, and the product was collected to obtain a polyurethane prepolymer;

[0072] Step 2: Add 4 g of 1,4-butanediol and 7 g of anti-aging additive to the polyurethane prepolymer, continue the reaction for 2.5 h, cool to 38 ° C, add 4.5 g of triethylamine to neutralize for 12 min, add 40 ml of deionized water, stir for 1.5 h, add 2.5 g of diisooctyl phthalate and 1.5 g of dimethyl silicone oil, stir well, and let stand to defoam to obtain a composite adhesive.

[0073] Comparative Example 5

[0074] Preparation of composite adhesive

[0075] Step 1: 25 g of isophorone diisocyanate, 18 g of polytetramethylene ether glycol, and 11 g of multi-performance rubber were mixed, nitrogen was introduced, 1.5 g of dibutyltin dilaurate was added, the mixture was stirred evenly, the temperature was raised to 62° C. and the mixture was reacted for 4 h, and the product was collected to obtain a polyurethane prepolymer;

[0076] Step 2: Add 4 g of 1,4-butanediol and 7 g of nano zinc oxide to the polyurethane prepolymer, continue the reaction for 2.5 h, cool to 38 ° C, add 4.5 g of triethylamine to neutralize for 12 min, add 40 ml of deionized water, stir for 1.5 h, add 2.5 g of diisooctyl phthalate and 1.5 g of dimethyl silicone oil, stir well, and let stand to defoam to obtain a composite adhesive.

[0077] Performance Testing

[0078] The composite adhesive prepared in Examples 1 to 3 and Comparative Examples 1 to 5 was coated on a steel plate that met the specifications, and cured at 80°C until dry to prepare a sample. The sample was placed at 200°C for 24 hours according to the reference standard GB / T1735-2009 to observe whether the sample morphology had any peeling or warping, and to test the high temperature resistance of the sample; the sample was placed in an accelerated aging box at 80°C, and after accelerated aging for 120 hours, the sample was torn open to observe the residual adhesive phenomenon and to determine the sample's resistance to thermal oxygen aging; the sample was subjected to a peel strength test according to the reference standard GB / T2792-2014, a sample treated in an ultraviolet aging box with a wavelength of 313nm and an irradiance of 0.72 / ㎡ for 24 hours, and a sample immersed in a hydrochloric acid solution with a concentration of 30% for 24 hours. The specific test results are shown in the following table:

[0079]

[0080] It can be seen from the above table that the composite adhesive prepared by using multi-performance rubber and anti-aging additives has excellent resistance to UV and thermal oxidation aging, excellent corrosion resistance and high temperature resistance, and high bonding strength. When used as an adhesive for reflective heat stickers, it can meet the use requirements of various fields and extend the service life of the reflective heat stickers.

[0081] The composite adhesive in Example 2 of the present invention is used to prepare a reflective heat transfer sticker, which specifically includes the following steps:

[0082] (1) The composite adhesive is evenly coated on one side of the polypropylene base film to a coating thickness of 20 μm, glass beads are evenly laid thereon, and a hot roller is used for extrusion and compaction at 100° C. to obtain a reflective layer;

[0083] (2) The composite adhesive was evenly coated on the other side of the polypropylene base film with a coating thickness of 25 μm, and cured at 80° C. for 15 min to form an adhesive layer, which was then covered with a silicone release film to obtain a PU reflective heat transfer sticker.

[0084] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0085] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the scope defined by the concept of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A method for making a PU reflective heat transfer sticker, characterized in that: The following steps are involved: (1) The composite adhesive is evenly coated on one side of the polypropylene base film, glass beads are evenly laid, and a hot roller is used for extrusion and compaction at 100-120° C. to obtain a reflective layer; (2) evenly coating the composite adhesive on the other side of the polypropylene base film, curing at 80-90° C. for 15-20 min to form an adhesive layer, and covering with a silicone release film to obtain a PU reflective heat transfer sticker; The coating thickness of the composite adhesive in the reflective layer is 20-25 μm; the coating thickness of the composite adhesive in the adhesive layer is 25-55 μm; The composite adhesive comprises the following raw materials in parts by weight: 20-30 parts of isophorone diisocyanate, 15-20 parts of polytetramethylene ether glycol, 10-12 parts of multi-performance rubber, 1-2 parts of dibutyltin dilaurate, 3-5 parts of 1,4-butanediol, 5-8 parts of anti-aging additives, 3-6 parts of triethylamine, 30-50 parts of deionized water, 2-3 parts of plasticizer, and 1-3 parts of defoaming agent.

2. The method for making a PU reflective heat transfer sticker according to claim 1, characterized in that: The plasticizer is diisononyl phthalate or diisooctyl phthalate; the defoamer is dimethyl silicone oil or polyethylene glycol.

3. The method for making a PU reflective heat transfer sticker according to claim 1, characterized in that: The preparation method of the multi-performance rubber comprises the following steps: S1: Put EPDM rubber in toluene, introduce nitrogen, add 4-maleimidobutyric acid and initiator, heat to 60-70°C and stir for 8-10h, collect the product after reduced pressure distillation, and obtain modified rubber; S2: Place the modified rubber and glycidyl furfuryl ether in N,N-dimethylformamide, mix thoroughly, add the catalyst, heat to 55-65°C and react for 6-8h, remove the solvent by rotary evaporation and collect the product to obtain a multi-performance rubber.

4. The method for making a PU reflective heat transfer sticker according to claim 3, characterized in that: In step S1, the initiator is benzoyl peroxide or dicumyl peroxide.

5. The method for making a PU reflective heat transfer sticker according to claim 3, characterized in that: In step S2, the catalyst is any one of tetrabutylammonium bromide, tetrabutylammonium hydrogen sulfate, and tetrabutylammonium hydroxide.

6. The method for making a PU reflective heat transfer sticker according to claim 1, characterized in that: The preparation method of the anti-aging additive comprises the following steps: SS1: Place nano zinc oxide in tetrahydrofuran, ultrasonically disperse for 15-20 minutes, add trimellitic anhydride formyl chloride and pyridine, place in an ice-water bath, let stand, filter, wash and dry to obtain modified nano zinc oxide; SS2: Place the modified nano zinc oxide in xylene, ultrasonically disperse for 10-15 minutes, add 3,5-di-tert-butyl-4-hydroxybenzyl alcohol and p-toluenesulfonic acid, heat to 55-70°C and react for 6-8 hours, filter, wash, dry and collect the product to obtain an anti-aging additive.

7. The method for making a PU reflective heat transfer sticker according to claim 6, characterized in that: In step SS1, the temperature of the ice water bath is 4-6°C and the time is 3-5h.

8. The method for making a PU reflective heat transfer sticker according to claim 1, characterized in that: The preparation method of the composite binder comprises the following steps: Step 1: Mix isophorone diisocyanate, polytetramethylene glycol, and multi-performance rubber, introduce nitrogen, add dibutyltin dilaurate, stir evenly, heat to 60-65° C. and react for 3-5 hours, and collect the product to obtain a polyurethane prepolymer; Step 2: Add 1,4-butanediol and anti-aging additives to the polyurethane prepolymer, continue to react for 2-3 hours, cool to 35-40°C, add triethylamine to neutralize for 10-15 minutes, add deionized water, stir for 1-2 hours, add plasticizer and defoamer, stir well, and let stand to defoam, to obtain a composite adhesive.

9. A PU reflective heat patch, characterized in that: The method is prepared by any one of claims 1 to 8.

Citation Information

Patent Citations

  • A high-brightness reflective adhesive composition for heat-sensitive adhesives and its preparation method

    CN114921201B