Covering hot melt adhesive as well as preparation method and application thereof
By using petroleum resin, antioxidants and metallocene catalytic polyolefins in the cover hot melt adhesive, combined with the stirring process, the problem of high-temperature use in the existing technology is solved, and efficient bonding is achieved at low temperatures is reduced. Carbide generation and shutdown rate are achieved, and excellent bonding strength is maintained.
Patent Information
- Application Number
- CN202411013140.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
AI Technical Summary
The existing hot-melt adhesive has a high temperature for use, resulting in high energy consumption, reduced efficiency of the glue cylinder, poor spraying of glue and reduced fitting strength, and insufficient bonding strength when used at low temperatures.
Hot melt adhesive with petroleum resin, antioxidants and metallocene catalytic polyolefins are used to reduce the melt viscosity and softening point through the stirring process. It is suitable for low-temperature operations and bonded at a temperature of 165℃-190℃. .
It effectively reduces the customer's operating temperature, reduces the production of carbides in the hot melt adhesive machine, improves the bonding strength and thermal stability, reduces the downtime and cleansing time, and maintains excellent bonding performance.
Smart Images

Figure BDA0004964965670000091
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of hot melt adhesives, and in particular to a covering hot melt adhesive and a preparation method and application thereof. Background Art
[0002] Hot melt adhesive is a plastic adhesive. Within a certain temperature range, the physical state of hot melt adhesive changes with temperature, while the chemical properties remain unchanged. Because the product itself is solid, does not contain any solvent, is non-toxic, dries quickly, has a simple production process, high economic benefits, requires little equipment investment, is easy to use, and has high production efficiency, hot melt adhesive is currently widely used in various industries, especially in the packaging field.
[0003] The existing hot melt adhesive for capping has a high operating temperature, generally at 210°C or above, which consumes more energy and is not in line with the future trend of energy conservation and carbon reduction. High operating temperature will also cause the hot melt adhesive to age more easily and produce gel or carbide. The produced gel and carbide adhere to the heated glue cylinder, reducing the heating efficiency of the glue cylinder. At the same time, it may also block the pipeline of the hot melt adhesive machine, causing the hot melt adhesive machine to spray glue unsmoothly, resulting in poor cap fitting. This will affect the efficiency and quality of cap fitting on the production line. If the operating temperature of the existing hot melt adhesive for capping is lowered, it will cause problems such as unsmooth glue spraying and reduced bonding strength. Summary of the invention
[0004] Based on this, it is necessary to provide a hot melt adhesive for covering, which has good shear strength, tensile strength, thermal stability and bonding strength, and can be suitable for operation at low temperatures.
[0005] The technical solution is as follows:
[0006] In a first aspect of the present invention, there is provided a hot melt adhesive for covering, wherein the raw materials thereof include the following components in parts by weight:
[0007] 30-60 parts of petroleum resin, 0.3-1.5 parts of antioxidant and 45-65 parts of metallocene-catalyzed polyolefin.
[0008] In one embodiment, the petroleum resin includes one or more of hydrogenated DCPD petroleum resin, hydrogenated C5 petroleum resin or hydrogenated C9 petroleum resin.
[0009] In one embodiment, the metallocene-catalyzed polyolefin includes one or more of a metallocene-catalyzed ethylene-propylene polymer, a metallocene-catalyzed ethylene-butene polymer, a metallocene-catalyzed propylene polymer, or a metallocene-catalyzed ethylene-octene polymer.
[0010] In one embodiment, the antioxidant includes one or more of antioxidant 1010 , antioxidant 168 , or antioxidant 1073 .
[0011] In one embodiment, the raw materials of the hot melt adhesive for covering further include 5-20 parts by weight of polyolefin block polymer.
[0012] In one embodiment, the polyolefin block polymer comprises a metallocene-catalyzed ethylene-octene block polymer.
[0013] A second aspect of the present invention provides a method for preparing the above-mentioned hot melt adhesive for covering, comprising the following steps:
[0014] Mixing the petroleum resin and the antioxidant, and stirring the obtained mixture for the first time;
[0015] The metallocene-catalyzed polyolefin and optionally the polyolefin block polymer are added to the mixture after the first stirring, and the mixture is stirred for the second time.
[0016] In one embodiment, the first stirring is performed at a temperature of 100° C. to 200° C.; and / or
[0017] The first stirring time is 15-25 minutes; and / or
[0018] The temperature for the second stirring is 100°C-200°C; and / or
[0019] The second stirring time is 50min-70min.
[0020] A third aspect of the present invention provides use of the above-mentioned lid-attaching hot-melt adhesive in attaching packaging boxes.
[0021] A fourth aspect of the present invention provides a packaging box laminating method, comprising the following steps:
[0022] Applying the lidding hot melt adhesive as described above to the packaging box to be attached;
[0023] The bonding is carried out at a temperature of 165°C-190°C.
[0024] Compared with the prior art, this application has the following beneficial effects:
[0025] The present application obtains a capping hot melt adhesive including components such as petroleum resin, antioxidant and metallocene catalyzed polyolefin by rationally designing the components of the capping hot melt adhesive. Experimental verification shows that the capping hot melt adhesive has good shear strength and tensile strength, effectively reduces the melt viscosity, thereby reducing the customer's operating temperature, reducing the generation of carbides in the hot melt machine, reducing the probability of clogging the hose and nozzle, and reducing the time of stopping to clean the glue cylinder; improving the thermal stability of the product, reducing the generation of carbides in the hot melt adhesive machine, and still having excellent bonding strength at a reduced operating temperature. In summary, the capping hot melt adhesive can solve the problems caused by high operating temperature while maintaining excellent bonding strength, and has good application potential in the bonding of beverage and dairy packaging lids. DETAILED DESCRIPTION
[0026] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.
[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0028] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0029] As used herein, "one or more" refers to any one, any two, or any two or more of the listed items.
[0030] Herein, the optional scope of "and / or", "or / and", and "and / or" includes any one of two or more relevant listed items, and also includes any and all combinations of the relevant listed items, wherein said any and all combinations include any two relevant listed items, any more relevant listed items, or a combination of all relevant listed items. (It should be noted that when at least three items are connected by at least two conjunctions selected from "and / or", "or / and", and "and / or", it should be understood that in the present application, the technical solution undoubtedly includes technical solutions that are all connected by "logical AND", and also undoubtedly includes technical solutions that are all connected by "logical OR". For example, "A and / or B" includes three parallel solutions of A, B and A+B. For another example, the technical solution of "A, and / or, B, and / or, C, and / or, D" includes any one of A, B, C, and D (that is, technical solutions that are all connected by "logical OR"), and also includes any and all combinations of A, B, C, and D, that is, a combination of any two or any three of A, B, C, and D, and also includes a combination of four items of A, B, C, and D (that is, a technical solution that is all connected by "logical AND").)
[0031] In this article, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0032] Herein, "further", "further", "particularly" and the like are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of this application.
[0033] Herein, "first aspect", "second aspect", "third aspect", "fourth aspect", etc. are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. In addition, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the description of the present application, the meaning of "several" is at least one, such as one, two, etc., unless otherwise clearly and specifically defined.
[0034] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0035] Only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an undefined range; and any lower limit can be combined with other lower limits to form an undefined range, and any upper limit can be combined with any other upper limit to form an undefined range. In addition, each separately disclosed point or single value itself can be combined with any other point or single value as a lower limit or upper limit or with other lower limits or upper limits to form an undefined range. The use of numerical ranges represented by endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4 and 5, etc.
[0036] The percentage contents involved in this application, unless otherwise specified, refer to mass percentage for solid-liquid mixing and solid-solid mixing, and refer to volume percentage for liquid-liquid mixing.
[0037] The percentage concentrations mentioned in this application, unless otherwise specified, refer to the final concentration, which refers to the percentage of the added component in the system after the addition of the component.
[0038] The temperature parameters in this application, unless otherwise specified, allow both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±2°C, ±1°C, ±0.5°C, ±0.4°C, ±0.3°C, ±0.2°C, and ±0.1°C are allowed. Normal temperature or room temperature in this application refers to no temperature control operation, generally 4°C to 35°C, preferably 20±5°C.
[0039] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0040] Hot melt adhesive, also known as hot melt adhesive, is an important category of adhesives. It has the characteristics of 100% solid content, no solvent, environmentally friendly and non-toxic, and fast curing. It is a plastic adhesive whose physical state changes with temperature, while the chemical properties remain unchanged. Hot melt adhesive is solid at room temperature. When heated to a certain temperature, it will melt into a viscous liquid. After coating and wetting the adherend, it is pressed and cooled to room temperature, and the bonding is completed within a few seconds. Hot melt adhesive has very strong viscosity in the molten state and can quickly bond various materials such as paper, wood, plastic, cloth, metal, etc. The existing hot melt adhesive for covering is used at a high temperature, generally at a temperature of 210°C or above. Most ordinary hot melt adhesives for covering use APAO (amorphous poly alpha olefin) as a polymer. APAO polymer has a wide molecular weight distribution and low crystallinity, and it is necessary to increase the molecular weight to provide better cohesion. The increase in molecular weight leads to high melt viscosity, and it is necessary to heat to a higher temperature during use, which leads to the production of carbides and clogging of hoses and nozzles. Based on this, the technicians of this application found through a lot of research that by selecting metallocene polyolefins, which have a narrow molecular weight distribution and a certain degree of crystallinity, the melt viscosity can be low under the condition of close cohesion, and the use temperature can be reduced. And the bonding strength of metallocene polyolefins to PP (the material of the lid) is better than that of APAO. Block polymers are selected in metallocene polyolefins, and block polymers have hard segments and soft segments. Hard segments can provide cohesion, and soft segments can provide better bonding strength.
[0041] In a first aspect of the present invention, there is provided a hot melt adhesive for covering, wherein the raw materials thereof include the following components in parts by weight:
[0042] 30-60 parts of petroleum resin, 0.3-1.5 parts of antioxidant and 45-65 parts of metallocene-catalyzed polyolefin.
[0043] In some examples, the petroleum resin includes one or more of hydrogenated DCPD petroleum resin, hydrogenated C5 petroleum resin or hydrogenated C9 petroleum resin.
[0044] In one specific example, the petroleum resin includes one or more of HM1000 or FM100.
[0045] In some examples, the metallocene-catalyzed polyolefin includes one or more of a metallocene-catalyzed ethylene-propylene polymer, a metallocene-catalyzed ethylene-butene polymer, a metallocene-catalyzed propylene polymer, or a metallocene-catalyzed ethylene-octene polymer.
[0046] In one specific example, the metallocene-catalyzed polyolefin includes one or more of GA1950, GA1900, GP1570 or DF7350.
[0047] In some examples, the antioxidant includes one or more of antioxidant 1010 , antioxidant 168 , or antioxidant 1073 .
[0048] In some examples, the raw materials of the hot melt adhesive for covering further include 5-20 parts of polyolefin block polymer by weight. It can be understood that the raw materials of the hot melt adhesive for covering further include 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20 parts of polyolefin block polymer by weight.
[0049] In some examples, the polyolefin block polymer includes a metallocene-catalyzed ethylene-octene block polymer.
[0050] A second aspect of the present invention provides a method for preparing the above-mentioned hot melt adhesive for covering, comprising the following steps:
[0051] Mixing the petroleum resin and the antioxidant, and stirring the obtained mixture for the first time;
[0052] The metallocene-catalyzed polyolefin and optionally the polyolefin block polymer are added to the mixture after the first stirring, and the mixture is stirred for the second time.
[0053] Specifically, the present application reduces the melt viscosity and softening point of the hot melt adhesive through polymer physical blending modification technology, so that the hot melt adhesive can lower the operating temperature; at the same time, it also improves the thermal stability at high temperature and is not easy to produce carbides; not only that, the modified hot melt adhesive improves the bonding strength to PP (the material of the lid), and even if the operating temperature is lowered, excellent bonding strength can be achieved.
[0054] In some examples, the temperature for the first stirring is 100° C.-200° C. It can be understood that the temperature for the first stirring includes but is not limited to 100° C., 102° C., 104° C., 106° C., 108° C., 110° C., 112° C., 114° C., 116° C., 118° C., 120° C., 122° C., 124° C., 126° C., 128° C., 130° C., 132° C., 134° C., 136° C., 138° C., 140° C., 142° C., 144° C., 146° C., 147° C., 148° C. 46℃, 148℃, 150℃, 152℃, 154℃, 156℃, 158℃, 160℃, 162℃, 164℃, 166℃, 168℃, 170℃, 172℃, 174℃, 176℃, 178℃, 180℃, 182℃, 184℃, 186℃, 188℃, 190℃, 192℃, 194℃, 196℃, 198℃, 200℃.
[0055] In some of these examples, the time for the first stirring is 15 min-25 min. It is understandable that the time for the first stirring includes but is not limited to 15 min, 15.5 min, 16 min, 16.5 min, 17 min, 17.5 min, 18 min, 18.5 min, 19 min, 19.5 min, 20 min, 20.5 min, 21 min, 21.5 min, 22 min, 22.5 min, 23 min, 23.5 min, 24 min, 24.5 min, 25 min.
[0056] In some examples, the temperature for the second stirring is 100° C.-200° C. It can be understood that the temperature for the second stirring includes but is not limited to 100° C., 102° C., 104° C., 106° C., 108° C., 110° C., 112° C., 114° C., 116° C., 118° C., 120° C., 122° C., 124° C., 126° C., 128° C., 130° C., 132° C., 134° C., 136° C., 138° C., 140° C., 142° C., 144° C., 146° C., 147° C., 148° C. 46℃, 148℃, 150℃, 152℃, 154℃, 156℃, 158℃, 160℃, 162℃, 164℃, 166℃, 168℃, 170℃, 172℃, 174℃, 176℃, 178℃, 180℃, 182℃, 184℃, 186℃, 188℃, 190℃, 192℃, 194℃, 196℃, 198℃, 200℃.
[0057] In some of these examples, the time for the second stirring is 50min-70min. It is understandable that the time for the second stirring includes but is not limited to 50min, 50.5min, 51min, 51.5min, 52min, 52.5min, 53min, 53.5min, 54min, 54.5min, 55min, 55.5min, 56min, 56.5min, 57min, 57.5min, 58min, 58.5min, 59min, 59.5min, 60min, 60.5min, 61min, 61.5min, 62min, 62.5min, 63min, 63.5min, 64min, 64.5min, 65min, 65.5min, 66min, 66.5min, 67min, 67.5min, 68min, 68.5min, 69min, 69.5min, 70min.
[0058] A third aspect of the present invention provides use of the above-mentioned lid-attaching hot-melt adhesive in attaching packaging boxes.
[0059] A fourth aspect of the present invention provides a packaging box laminating method, comprising the following steps:
[0060] Applying the lidding hot melt adhesive as described above to the packaging box to be attached;
[0061] The bonding is carried out at a temperature of 165°C-190°C.
[0062] The present application obtains a capping hot melt adhesive including components such as petroleum resin, antioxidant and metallocene catalyzed polyolefin by rationally designing the components of the capping hot melt adhesive. Experimental verification shows that the capping hot melt adhesive has good shear strength and tensile strength, effectively reduces the melt viscosity, thereby reducing the customer's operating temperature, reducing the generation of carbides in the hot melt machine, reducing the probability of clogging the hose and nozzle, and reducing the time of stopping to clean the glue cylinder; improving the thermal stability of the product, reducing the generation of carbides in the hot melt adhesive machine, and still having excellent bonding strength at a reduced operating temperature. In summary, the capping hot melt adhesive can solve the problems caused by high operating temperature while maintaining excellent bonding strength, and has good application potential in the bonding of beverage and dairy packaging lids.
[0063] The present application is further described in detail below in conjunction with specific examples. For experimental parameters not specified in the following specific examples, reference is made to the instructions given in the present application document, and reference may also be made to the experimental manual of the art or other experimental methods known in the art, or to the experimental conditions recommended by the manufacturer. It is understood that the instruments and raw materials used in the following examples are relatively specific, and may not be limited thereto in other specific examples.
[0064] Some of the raw materials used in the embodiment are as follows:
[0065] The petroleum resins are specifically HM1000 and FM100, which can be purchased from Henghe Materials Technology Co., Ltd. and Lianchao Industrial Co., Ltd.;
[0066] The antioxidants are specifically antioxidant 1010 and antioxidant 168, which can be purchased from Tianjin Lianlong New Materials Co., Ltd.;
[0067] Metallocene-catalyzed polyolefins are specifically GA1950, GA1900, GP1570, and DF7350, which can be purchased from DOW and Mitsui Chemicals;
[0068] The polyolefin block polymers are specifically available from DOW;
[0069] Metallocene-catalyzed ethylene propylene polymers are available from EXXON;
[0070] APAO polymers are available from Evonik;
[0071] PE wax can be purchased from Clariant;
[0072] PP wax is available from Clariant.
[0073] The following are specific embodiments.
[0074] Example 1
[0075] Add 40 parts of petroleum resin (hydrogenated DCPD petroleum resin) and 0.5 parts of antioxidant (1010) into the reactor, heat to 150°C, stir and melt for 20 minutes; add 30 parts of metallocene-catalyzed ethylene-propylene polymer, 15 parts of metallocene-catalyzed ethylene-octene polymer and 15 parts of polyolefin block polymer (metallocene-catalyzed ethylene-octene block polymer), add materials at intervals, and add materials in 3 times. After the polymer is melted, vacuum and stir for 60 minutes at a stirring temperature of 150°C. After observing that there are no bubbles, the material can be discharged.
[0076] Example 2
[0077] Add 40 parts of petroleum resin (hydrogenated DCPD petroleum resin) and 0.5 parts of antioxidant (0.3 parts of antioxidant 1010 and 0.2 parts of antioxidant 168) into the reactor, heat to 150°C, stir and melt for 20 minutes; add 60 parts of metallocene-catalyzed ethylene octene polymer, add the materials at intervals, and add the materials in 3 times. After the polymer is melted, vacuum and stir for 60 minutes at a stirring temperature of 150°C. After observing that there are no bubbles, the material can be discharged.
[0078] Example 3
[0079] Add 40 parts of petroleum resin (hydrogenated C9 petroleum resin) and 0.5 parts of antioxidant (0.3 parts of antioxidant 1010 and 0.2 parts of antioxidant 168) to the reactor, heat to 150°C, stir and melt for 20 minutes; add 15 parts of metallocene-catalyzed ethylene octene polymer and 45 parts of metallocene-catalyzed ethylene propylene polymer, add materials at intervals, and add materials in 3 times. After the polymer is melted, vacuum and stir for 60 minutes at a stirring temperature of 150°C. After observing that there are no bubbles, the material can be discharged.
[0080] Comparative Example 1
[0081] 37 parts of petroleum resin (hydrogenated C9 petroleum resin), 0.5 parts of antioxidant 1010 and 0.5 parts of antioxidant 1073 were added to the reactor, heated to 150°C, and stirred to melt for 20 minutes; 63 parts of APAO polymer were added, and the temperature was raised to 180°C at intervals, and the materials were added in 3 times. After the polymer was melted, vacuum stirred for 60 minutes at a stirring temperature of 165°C, and the material was discharged after no bubbles were observed.
[0082] Comparative Example 2
[0083] Add 30 parts of petroleum resin (hydrogenated DCPD petroleum resin) and 0.5 parts of antioxidant (0.3 parts of antioxidant 1010 and 0.2 parts of antioxidant 168) to the reactor, heat to 150°C, stir and melt for 20 minutes; add 10 parts of metallocene-catalyzed ethylene-octene polymer and 45 parts of metallocene-catalyzed ethylene-propylene polymer, feed at intervals, and feed in 3 times. Add 10 parts of PE wax and 5 parts of PP wax, and heat to 180°C. After the polymer is melted, vacuum and stir for 60 minutes, and discharge after observing that there are no bubbles.
[0084] The hot melt adhesives prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were subjected to performance tests such as melt viscosity at 25°C, shear strength at 25°C, tensile strength at 0°C, tensile strength at -10°C, thermal stability, and rate of change of hot melt viscosity after heating for 8 hours. The test results are shown in Table 1 below.
[0085] Table 1
[0086]
[0087] As can be seen from Table 1 above, the shear strength of Examples 1, 2 and 3 on PP materials is better than that of Comparative Example 1; at the set use temperature, the appearance color of Examples 1, 2 and 3 changes little, no carbide is produced, the melt viscosity remains stable, and the thermal stability is significantly better than that of Comparative Example 1. The low-temperature strength of Examples 1, 2 and 3 on PP materials is better than that of Comparative Example 2.
[0088] In summary, the thermal stability of comparative example 1 is poor, and the cold resistance of comparative example 2 is poor. The embodiment has made improvements in these two aspects: the present application effectively reduces the melt viscosity, thereby reducing the customer's operating temperature, reducing the generation of carbides in the hot melt machine, reducing the probability of clogging the hose and nozzle, and reducing the time of stopping to clean the glue cylinder; the present application also improves the thermal stability of the product and reduces the generation of carbides in the hot melt adhesive machine. The present application still has excellent bonding strength at a reduced operating temperature. In summary, the present application solves the problem caused by the high operating temperature of the old solution while maintaining excellent bonding strength.
[0089] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0090] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims, and the description may be used to interpret the content of the claims.
Claims
1. A hot melt adhesive for covering, characterized in that: The raw materials include the following components by weight: 30-60 parts of petroleum resin, 0.3-1.5 parts of antioxidant and 45-65 parts of metallocene-catalyzed polyolefin.
2. The hot melt adhesive for covering according to claim 1, characterized in that: The petroleum resin includes one or more of hydrogenated DCPD petroleum resin, hydrogenated C5 petroleum resin or hydrogenated C9 petroleum resin.
3. The hot melt adhesive for covering according to claim 1, characterized in that: The metallocene-catalyzed polyolefin includes one or more of a metallocene-catalyzed ethylene-propylene polymer, a metallocene-catalyzed ethylene-butene polymer, a metallocene-catalyzed propylene polymer or a metallocene-catalyzed ethylene-octene polymer.
4. The hot melt adhesive for covering according to claim 1, characterized in that: The antioxidant includes one or more of antioxidant 1010 , antioxidant 168 , or antioxidant 1073 .
5. The hot melt adhesive for covering according to any one of claims 1 to 4, characterized in that: The raw materials also include 5-20 parts of polyolefin block polymer by weight.
6. The hot melt adhesive for covering according to claim 5, characterized in that: The polyolefin block polymer includes a metallocene-catalyzed ethylene-octene block polymer.
7. A method for preparing the hot melt adhesive for covering according to any one of claims 1 to 6, characterized in that: The following steps are involved: Mixing the petroleum resin and the antioxidant, and stirring the obtained mixture for the first time; The metallocene-catalyzed polyolefin and optionally the polyolefin block polymer are added to the mixture after the first stirring, and the mixture is stirred for the second time.
8. The method for preparing the hot melt adhesive for covering according to claim 7, characterized in that: The temperature for the first stirring is 100°C-200°C; and / or The first stirring time is 15-25 minutes; and / or The temperature for the second stirring is 100°C-200°C; and / or The second stirring time is 50min-70min.
9. Use of the lid-sticking hot-melt adhesive according to any one of claims 1 to 6 in sticking packaging boxes.
10. A packaging box laminating method, characterized in that: The steps include: Applying the lid-sticking hot melt adhesive according to any one of claims 1 to 6 to the packaging box to be attached; The bonding is carried out at a temperature of 165°C-190°C.