Production process of high-cleanliness ultra-low carbon steel
Through the RH+VOD dual-control process, combined with top-blowing hydrogen and bottom-blowing hydrogen, the liquid steel and slag surface deoxidation is solved, and the production of high-cleanness ultra-low carbon steel is achieved. It reduces iron loss and alloy oxidation consumption, and improves the cleanliness and mechanical properties of the steel.
Patent Information
- Application Number
- CN202410997273.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-24
AI Technical Summary
In the production process of ultra-low carbon steel, the use of top slag modified agent in the prior art has inaccurate amount of addition, which leads to large fluctuations in the total iron content of top slag, which may cause smoke pollution, difficulty in mixing and excessive increase in FeO content. Iron damage problem.
Using the RH+VOD dual-control process, after RH decarbonization treatment, blow hydrogen in the lower top gun in the VOD furnace and blow hydrogen in the bottom breathable brick to deoxygenate the liquid steel and slag surfaces, avoid the use of deoxygenation alloy, alloying, and controlling the vacuum degree and gas blowing strength to achieve high cleanliness of liquid steel production.
Improves the cleanliness of the molten steel, reduces the secondary oxidation of the molten steel by slag, increases the recovery rate of Fe in the slag, reduces iron loss, improves the alloy yield and the mechanical properties of the molten steel, and is suitable for automotive lightweighting. need.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of iron and steel metallurgy, and specifically relates to a production process for high-cleanliness ultra-low carbon steel. Background Art
[0002] In the production process of ultra-low carbon steel, some scholars have proposed to use hydrogen deoxidation in the refining steps of AOD, RH, and RH+VD. This clean deoxidation method avoids the formation of oxide inclusions. However, due to the diffusion of oxygen between the slag and steel interface, when the oxygen content is lower than the slag / steel oxygen content equilibrium point, the steel transfers oxygen to the slag to achieve diffusion deoxidation, while when the oxygen content is higher than the slag / steel oxygen content equilibrium point, the slag transfers oxygen to the steel, and secondary oxidation occurs. Clean deoxidation methods such as hydrogen deoxidation can reduce the oxygen content to a lower level, but if the oxygen content in the slag is not stably controlled, it may lead to poor control of the final oxygen content. At present, when using top slag modifiers, there are still some problems that cannot be avoided under the existing technology:
[0003] (1) When the top slag is pre-deoxidized with a pre-deoxidizer, if the amount added is too little, the slag cannot be pre-deoxidized efficiently. If the amount added is too much, it will not only affect the fluidity and other properties of the refined slag, but also cause Al2O3 to diffuse into the molten steel;
[0004] (2) After the steel is tapped, adding a modifier to the ladle slag surface may generate smoke and pollute the environment;
[0005] (3) Imprecise calculation of the amount of modifier added will lead to large fluctuations in the total iron content of the ladle top slag;
[0006] (4) After the RH immersion tube is lowered, the slag layer is thick, and it is difficult to mix after adding the top slag modifier. Bottom blowing may cause the molten steel to be exposed, and the mixing effect is poor if the bottom blowing flow rate is not enough;
[0007] (5) If the FeO content in the slag is too high, it will increase iron loss. Summary of the invention
[0008] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a production process for high-cleanliness ultra-low carbon steel.
[0009] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:
[0010] A production process for ultra-low carbon steel with high cleanliness. Through RH+VOD dual control, the molten steel is decarburized by RH and then sent to the VOD furnace. After the VOD reaches the vacuum requirement, a top gun is lowered to the slag surface to blow hydrogen, and air is blown through the bottom air bricks at the same time. The bottom hydrogen is blown to deoxidize the molten steel, and the top hydrogen is blown on the slag surface to deoxidize the steel slag and modify the top slag at the same time. After breaking the air, alloying is carried out, and no deoxidizing alloy is used in the process.
[0011] As a preferred solution of the production process of high-cleanliness ultra-low carbon steel described in the present invention, the production process specifically includes: KR pretreatment, converter smelting, RH, VOD, and continuous casting.
[0012] As a preferred solution of the production process of high-cleanliness ultra-low carbon steel described in the present invention, wherein: KR pretreatment is used for hot metal desulfurization, and the [S] content in the hot metal after treatment is required to be ≤50×10 -6 .
[0013] As a preferred solution of the production process of high-cleanliness ultra-low carbon steel described in the present invention, wherein: the scrap steel ratio of the converter is controlled to be ≤22%; the FeO content at the end of blowing is 22wt%; the converter end temperature is required to be controlled at 1690-1710°C, and the end point [C] content is controlled at (320-480)×10 -6 , end point [P] content ≤ 90 × 10 -6 , end point [S] content ≤ 55 × 10 -6 , end point [O] content ≥480×10 -6 ; Steel is tapped using a carbon-free ladle; 0.8-3.5kg / t of steel is added 钢 of lime.
[0014] As a preferred solution of the production process of high-cleanliness ultra-low carbon steel described in the present invention, the ladle car is driven to the RH station, and vacuum is started to start the circulation; a five-stage or four-stage vacuum pump is used to vacuum to 5-15kPa to maintain the vacuum degree, and the lower oxygen lance starts forced decarburization, and the oxygen blowing intensity is 1200-4200NL / t 钢 / min, oxygen blowing time is 5 to 18min; after decarburization, the third-stage pump, the second-stage pump, and the first-stage pump are started in sequence at intervals of 1min. After the first-stage pump is started, the vacuum degree of the vacuum chamber is maintained at ≤67Pa, and the vacuum degree is maintained for 5 to 20min for natural decarburization; after decarburization, the vacuum chamber is opened and the station is exited. The exit requirement is [C] content ≤15×10 -6 , the molten steel temperature is required to be 1662~1688℃.
[0015] As a preferred solution of the production process of high-cleanliness ultra-low carbon steel described in the present invention, no top slag modifier is added after the RH leaves the station, and it is directly sent to the VOD station.
[0016] As a preferred solution of the production process of high-cleanliness ultra-low carbon steel described in the present invention, wherein: after entering the VOD station, the ladle is covered and vacuum treatment begins. When the vacuum degree reaches 1500-3500Pa, the lower top gun is placed above the slag surface, and a hydrogen-inert gas mixture with a hydrogen ratio of 10-50% is sprayed, and the spraying intensity is 1500-4500NL / t 钢 / min, the blowing time is 8 to 20min; at the same time, a hydrogen-inert gas mixture with a hydrogen ratio of 10 to 50% is blown into the bottom through the bottom air bricks, and multiple bottom blowing holes can be selected for bottom blowing, with a total gas supply intensity of 1200 to 6000NL / t 钢 / min, the blowing time is 8 to 30min; when the blowing volume reaches 50%, the vacuum degree continues to be reduced. When the hydrogen blowing is finished, the vacuum degree of the vacuum chamber is adjusted to ≤67Pa. Bottom-blown air-permeable bricks are used to blow argon into the molten steel to assist in degassing. The total gas supply intensity is 1200 to 4500NL / t 钢 / min, the blowing time is 5 to 15min; VOD outbound requirements are that the molten steel temperature is 1585 to 1630℃, and the molten steel [C] content is ≤15×10 -6 , [O] content ≤ 15×10 -6 , [P] content ≤ 90 × 10 -6 , [N] content ≤ 30 × 10 -6 , [H] content ≤ 3 × 10 -6 , [S] content ≤ 50 × 10 -6 .
[0017] As a preferred solution of the production process of high-cleanliness ultra-low carbon steel described in the present invention, the amount of alloy to be added is calculated according to the composition of the molten steel tapped by VOD; soft blowing is performed for 5 to 10 minutes after the alloy is added to ensure uniform composition of the molten steel; after alloying, the temperature of the molten steel is required to be controlled at 1570 to 1595°C, and the [C] content in the molten steel is ≤15×10 -6 , [Si] content ≤ 55 × 10 -6 , [Mn] content is (900-1300)×10 -6 , [P] content ≤ 90 × 10 -6 , [S] content ≤ 50 × 10 -6 , [Ti] content ≤ 110×10 -6 , [Als] content ≤ 15×10 -6 , [O] content ≤ 15×10 -6 , [N] content ≤ 30 × 10 -6 , [H] content ≤ 3 × 10 -6 .
[0018] As a preferred solution of the production process of high-cleanliness ultra-low carbon steel described in the present invention, wherein: protective casting measures are adopted in continuous casting to strictly prevent secondary oxidation of molten steel and control the temperature of the tundish at 1554-1570°C; ultra-low carbon covering agent is used as the crystallizer covering agent, and protective casting is performed during the whole continuous casting process, and the process requires oxygen addition of less than 3×10 -6 , nitrogen addition is less than 3×10 -6 .
[0019] The beneficial effects of the present invention are as follows:
[0020] The present invention proposes a production process of ultra-low carbon steel with high cleanliness. Through RH+VOD dual control, the molten steel is decarburized by RH and then sent to the VOD furnace. After the VOD reaches the vacuum requirement, a top gun is used to blow hydrogen to the slag surface, and air is blown through the bottom air-permeable bricks. The bottom hydrogen is blown to deoxidize the molten steel, and the top hydrogen is blown on the slag surface to deoxidize the steel slag and modify the top slag at the same time. After breaking the air, alloying is performed, and no deoxidized alloy is used in the process. The present invention has high safety and effective treatment of gas emissions; the top hydrogen blowing reduces the slag oxidation and reduces the secondary oxidation of the slag to the molten steel; the recovery rate of Fe in the slag is increased and the iron loss is reduced; the low oxygen condition increases the alloy recovery rate and reduces the alloy oxidation consumption; the good kinetic conditions are conducive to the efficient floating of inclusions in the molten steel; the cleanliness of the molten steel is significantly improved, which is conducive to the improvement of the mechanical properties of the steel and the lightweight of the automobile. DETAILED DESCRIPTION
[0021] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] The present invention provides a production process of ultra-low carbon steel with high cleanliness, which is a method for pre-deoxidation without using deoxidation alloys such as aluminum particles, pre-melted slag, etc., and can reduce iron loss and increase the recovery rate of iron in slag. The clean top slag pre-deoxidation process is combined with the clean deoxidation process to produce ultra-low carbon steel with high cleanliness. The process of using reducing gas to carry out efficient deoxidation of molten steel and combining it with the top slag pre-deoxidation process can not only achieve efficient deoxidation of molten steel, but also increase the recovery rate of iron in slag. The blowing of gas improves the kinetic conditions of slag, which is conducive to the deoxidation reaction. The reduction product is pollution-free H2O gas, which can also effectively reduce the oxidizability in slag and avoid secondary oxidation of molten steel. VOD has the degassing ability to remove residual H and N.
[0023] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0024] Example 1
[0025] This embodiment is a production process of high-cleanliness IF steel, comprising the following steps:
[0026] (1) KR pretreatment is used for hot metal desulfurization, and the [S] content in the hot metal after treatment is required to be 46×10 -6 .
[0027] (2) The scrap ratio of the converter was controlled to be 15%; the FeO content at the end of blowing was 24wt%, the final converter temperature was controlled at 1703℃, the molten steel volume was 198t, and the final [C] content was controlled at 340×10 -6 The end point [P] content is 86×10 -6 The final [S] content is 48×10 -6 The final [O] content is 688×10 -6 ; Steel is tapped using a carbon-free ladle; 436kg of lime is added during steel tapping.
[0028] (3) Drive the ladle car to the RH station, measure the temperature to 1688℃, and set the oxygen to 662×10 -6 ; Start to evacuate and start circulation; Use a five-stage or four-stage vacuum pump to evacuate to 10kPa to maintain the vacuum degree, and start forced decarburization with the lower oxygen gun, and the oxygen blowing intensity is 1500NL / t 钢 / min, oxygen blowing time is 13min; after decarburization, the third-stage pump, the second-stage pump, and the first-stage pump are started in turn at intervals of 1min. After the first-stage pump is started, the vacuum degree of the vacuum chamber is maintained at 67Pa, and the vacuum degree is maintained for 10min for natural decarburization; after decarburization, the vacuum chamber is broken out of the station, and the outbound [C] content is 13×10 -6 , [O] content is 506×10 -6 , the FeO content of the top slag is 27wt%, and the molten steel temperature is 1665℃.
[0029] (4) After RH leaves the station, no top slag modifier is added and it is directly sent to the VOD station. After entering the VOD station, the ladle is covered and vacuum treatment begins. When the vacuum degree reaches 3000Pa, the top gun is placed above the slag surface and a hydrogen-argon mixed gas with a hydrogen ratio of 30% is sprayed at a spray intensity of 2200NL / t 钢 / min, the blowing time is 12min; at the same time, a hydrogen-argon mixed gas with a hydrogen ratio of 30% is blown into the bottom air brick, and the total gas supply intensity is 1800NL / t 钢 / min, the blowing time is 20min; when the blowing volume reaches 50%, the vacuum degree continues to be reduced. When the hydrogen blowing is finished, the vacuum degree of the vacuum chamber is adjusted to 67Pa. The bottom blowing air brick is used to blow argon into the molten steel to assist in degassing. The total gas supply intensity is 2000NL / t 钢 / min, the blowing time is 12min; the temperature of the molten steel out of the VOD station is 1610℃, and the [C] content of the molten steel is 13×10 -6 , [O] content is 9×10 -6 , [P] content 88×10 -6 , [N] content 28×10 -6 , [H] content 2.5×10 -6 , [S] content 45×10 -6The amount of alloy to be added was calculated based on the composition of the molten steel tapped by VOD. After the alloy was added, soft blowing was performed for 7 minutes to ensure uniform composition of the molten steel. After alloying, the temperature of the molten steel was controlled at 1588°C, and the [C] content in the molten steel was 13×10 -6 , [Si] content is 52×10 -6 , [Mn] content is 932×10 -6 , [P] content is 88×10 -6 , [S] content is 45×10 -6 , [Ti] content is 102×10 -6 , [Als] content is 12×10 -6 , [O] content is 13×10 -6 , [N] content is 24×10 -6 , [H] content is 2.2×10 -6 .
[0030] (5) Protective casting measures are taken during continuous casting to strictly prevent secondary oxidation of molten steel and control the tundish temperature at 1556-1568°C; ultra-low carbon covering agent is used for the crystallizer covering agent, and protective casting is performed throughout the continuous casting process. The process requires oxygen addition of less than 3×10 -6 , nitrogen addition is less than 3×10 -6 .
[0031] The ingot prepared in Example 1 was sampled and the sample inclusions were detected by using the ASPEX inclusion automatic scanning system. The number density of inclusions larger than 1 μm was found to be 4 / mm. 2 , the average size of inclusions is 1.5μm.
[0032] Example 2
[0033] This embodiment is a production process of high-cleanliness IF steel, comprising the following steps:
[0034] (1) KR pretreatment is used for hot metal desulfurization, and the [S] content in the hot metal after treatment is required to be 36×10 -6 .
[0035] (2) The scrap ratio of the converter is controlled to be 21%; the FeO content at the end of blowing is 21wt%, the converter end temperature is required to be controlled at 1698℃, the molten steel volume is 122t, and the end [C] content is controlled at 330×10 -6 The end point [P] content is 85×10 -6 , the end point [S] content is 47×10 -6 The end point [O] content is 697×10 -6 ; Steel is tapped using a carbon-free ladle; 313kg of lime is added during steel tapping.
[0036] (3) Drive the ladle car to the RH station, measure the temperature to 1679°C, and set the oxygen to 661×10 -6 , start to evacuate and start circulation; use a five-stage or four-stage vacuum pump to evacuate to 8kPa to maintain the vacuum degree, and the lower oxygen gun starts forced decarburization, and the oxygen supply intensity is 1600NL / t 钢 / min, oxygen blowing time is 12min; after decarburization, the third-stage pump, the second-stage pump, and the first-stage pump are started in turn at intervals of 1min. After the first-stage pump is started, the vacuum degree of the vacuum chamber is maintained at 67Pa, and the vacuum degree is maintained for 11min for natural decarburization; after decarburization, the vacuum chamber is broken out of the station, and the outbound [C] content is 11×10 -6 , [O] content is 403×10 -6 , molten steel temperature is 1663℃.
[0037] (4) After RH leaves the station, no top slag modifier is added and it is directly sent to the VOD station. After entering the VOD station, the ladle is covered and vacuum treatment begins. When the vacuum degree reaches 2800Pa, the top gun is placed above the slag surface and a hydrogen-argon mixed gas with a hydrogen ratio of 20% is sprayed at a spray intensity of 1800NL / t 钢 / min, the blowing time is 14min; at the same time, a hydrogen-argon mixed gas with a hydrogen ratio of 20% is blown into the bottom air brick, and the total gas supply intensity is 2400NL / t 钢 / min, the blowing time is 24min; when the blowing volume reaches 50%, the vacuum degree continues to be reduced. When the hydrogen blowing is finished, the vacuum degree of the vacuum chamber is adjusted to 67Pa. Bottom-blown air-permeable bricks are used to blow argon into the molten steel to assist in degassing. The total gas supply intensity is 2100NL / t 钢 / min, the blowing time is 9min; the temperature of the molten steel out of the VOD station is 1629℃, and the [C] content of the molten steel is 14×10 -6 , [O] content is 12×10 -6 , [P] content 89×10 -6 , [N] content 26×10 -6 , [H] content 2×10 -6 , [S] content 44×10 -6 According to the calculation of the VOD steel liquid composition, the amount of alloy to be added is calculated; after the alloy is added, soft blowing is performed for 6 minutes to ensure uniform composition of the steel liquid; after alloying, the temperature of the steel liquid is required to be controlled at 1591°C, and the [C] content in the steel liquid is 12×10 -6 , [Si] content is 50×10 -6 , [Mn] content is 1013×10 -6 , [P] content is 88×10 -6 , [S] content is 33×10 -6 , [Ti] content is 95×10 -6 , [Als] content is 10×10 -6, [O] content is 14×10 -6 , [N] content is 27×10 -6 , [H] content is 2×10 -6 .
[0038] (5) Protective casting measures are taken during continuous casting to strictly prevent secondary oxidation of molten steel and control the tundish temperature at 1554-1569°C; ultra-low carbon covering agent is used for the crystallizer covering agent, and protective casting is performed throughout the continuous casting process. The process requires oxygen addition of less than 3×10 -6 , nitrogen addition is less than 3×10 -6 .
[0039] The ingot prepared in Example 2 was sampled and the sample inclusions were detected by using the ASPEX inclusion automatic scanning system. The number density of inclusions larger than 1 μm was found to be 4.3 / mm. 2 , the average size of inclusions is 1.8μm.
[0040] Comparative Example 1
[0041] This comparative example is a production process of IF steel, comprising the following steps:
[0042] (1) KR pretreatment is used for hot metal desulfurization, and the [S] content in the hot metal after treatment is required to be 43×10 -6 .
[0043] (2) The scrap ratio of the converter was controlled at 21%; the FeO content at the end of blowing was 24wt%, the converter terminal temperature was controlled at 1699°C, the molten steel volume was 205t, and the terminal [C] content was controlled at 312×10 -6 The end point [P] content is 86×10 -6 The final [S] content is 47×10 -6 The final [O] content is 714×10 -6 ; Steel is tapped using a carbon-free ladle; 496kg of lime is added during steel tapping.
[0044] (3) Drive the ladle car to the RH station, measure the temperature to 1679°C, and set the oxygen to 682×10 -6 ; Start to evacuate and start circulation; Use a five-stage or four-stage vacuum pump to evacuate to 10kPa to maintain the vacuum degree, and start forced decarburization with the lower oxygen gun, and the oxygen blowing intensity is 2200NL / t 钢 / min, oxygen blowing time is 11min; after decarburization, 182kg aluminum-containing top slag modifier is added, and then the third-stage pump, second-stage pump, and first-stage pump are turned on in sequence at intervals of 1min. After turning on the first-stage pump, the vacuum degree of the vacuum chamber is maintained at 67Pa, and the vacuum degree is maintained for 6min for natural decarburization; after decarburization, deoxidizer is added according to the oxygen determination result, and after circulating for 3min, alloy is added according to the test result for alloying, and the alloy composition is adjusted and circulated for 6min before breaking out of the station; the RH exit molten steel temperature is 1594℃, and the [C] content in the molten steel is 14×10 -6 , [Si] content is 54×10 -6 , [Mn] content is 1011×10 -6 , [P] content is 88×10 -6 , [S] content is 47×10 -6 , [Ti] content is 106×10 -6 , [Als] content is 29×10 -6 , [O] content is 23×10 -6 , [N] content is 25×10 -6 , [H] content is 2×10 -6 .
[0045] (5) Protective casting measures are taken during continuous casting to strictly prevent secondary oxidation of molten steel and control the tundish temperature at 1558-1569°C; ultra-low carbon covering agent is used for the crystallizer covering agent, and protective casting is performed throughout the continuous casting process. The process requires oxygen addition of less than 3×10 -6 , nitrogen addition is less than 3×10 -6 .
[0046] The ingots prepared in Comparative Example 1 were sampled and the inclusions in the samples were detected by using the ASPEX inclusion automatic scanning system. The statistical result showed that the number density of inclusions larger than 1 μm was 10.3 / mm. 2 , the average size of inclusions is 4.1μm.
[0047] Comparative Example 2
[0048] This comparative example is a production process of IF steel RH+VOD, comprising the following steps:
[0049] (1) KR pretreatment is used for hot metal desulfurization, and the [S] content in the hot metal after treatment is required to be 43×10 -6 .
[0050] (2) The scrap ratio of the converter is controlled to be 18%; the FeO content at the end of blowing is 20wt%, the converter end temperature is required to be controlled at 1701℃, the molten steel volume is 125t, and the end [C] content is controlled at 341×10 -6 The end point [P] content is 86×10 -6, end point [S] content 45×10 -6 The final [O] content is 693×10 -6 ; Steel is tapped using a carbon-free ladle; 288kg of lime is added during steel tapping.
[0051] (3) Drive the ladle car to the RH station, measure the temperature to 1683℃, and set the oxygen to 671×10 -6 , start to evacuate and start circulation; use a five-stage or four-stage vacuum pump to evacuate to 10kPa to maintain the vacuum degree, and the lower oxygen gun starts forced decarburization, and the oxygen supply intensity is 1800NL / t 钢 / min, oxygen blowing time is 13min; after decarburization, the third-stage pump, the second-stage pump, and the first-stage pump are turned on in sequence at intervals of 1min. After the first-stage pump is turned on, the vacuum degree of the vacuum chamber is maintained at 67Pa, and the vacuum degree is maintained for 13min for natural decarburization; after decarburization, the vacuum chamber is broken out of the station, and the outbound [C] content is 13×10 -6 , [O] content is 413×10 -6 , molten steel temperature is 1663℃.
[0052] (4) RH is directly sent to the VOD station after leaving the station. After entering the VOD station, the ladle is covered and vacuum treatment begins. When the vacuum degree reaches 3000Pa, the top gun is placed above the slag surface and a hydrogen-argon mixed gas with a hydrogen ratio of 10% is sprayed at a spray intensity of 1200NL / t. 钢 / min, the blowing time is 6min; at the same time, a hydrogen-argon mixed gas with a hydrogen ratio of 10% is blown into the bottom air brick, and the total gas supply intensity is 1600NL / t 钢 / min, the blowing time is 17min; the vacuum degree continues to be reduced at the end of top blowing, and the vacuum degree of the vacuum chamber is adjusted to 67Pa at the end of hydrogen blowing. Argon is blown into the molten steel using bottom blowing air bricks to assist in degassing. The total gas supply intensity is 2100NL / t 钢 / min, the blowing time is 10min; the temperature of the molten steel out of the VOD station is 1618℃, and the [C] content of the molten steel is 13×10 -6 , [O] content is 25×10 -6 , [P] content 88×10 -6 , [N] content 25×10 -6 , [H] content 3×10 -6 , [S] content 43×10 -6 The amount of alloy to be added is calculated based on the composition of the molten steel tapped by VOD. After the alloy is added, soft blowing is performed for 6 minutes to ensure uniform composition of the molten steel. After alloying, the temperature of the molten steel is 1591°C, and the [C] content in the molten steel is 15×10 -6 , [Si] content is 54×10 -6 , [Mn] content is 1094×10 -6 , [P] content is 85×10-6 , [S] content is 44×10 -6 , [Ti] content is 102×10 -6 , [Als] content is 13×10 -6 , [O] content is 28×10 -6 , [N] content is 27×10 -6 , [H] content is 3×10 -6 .
[0053] (5) Protective casting measures are taken during continuous casting to strictly prevent secondary oxidation of molten steel and control the tundish temperature at 1557-1566°C; ultra-low carbon covering agent is used for the crystallizer covering agent, and protective casting is performed throughout the continuous casting process. The process requires oxygen addition of less than 3×10 -6 , nitrogen addition is less than 3×10 -6 .
[0054] The ingots prepared in Comparative Example 2 were sampled and the inclusions in the samples were detected by using the ASPEX inclusion automatic scanning system. The number density of inclusions larger than 1 μm was found to be 6.3 / mm. 2 , the average size of inclusions is 3.5μm.
[0055] The present invention uses RH+VOD dual control. The molten steel is treated with RH decarburization and then sent to the VOD furnace. After the VOD reaches the vacuum requirement, a top gun is used to blow hydrogen to the slag surface. At the same time, air is blown through the bottom air-permeable bricks. The bottom blows hydrogen to deoxidize the molten steel. The top blows hydrogen to deoxidize the steel slag and modify the top slag. After breaking the air, alloying is performed, and no deoxidized alloy is used in the process. The present invention has high safety and effective treatment of gas emissions. The top blowing of hydrogen reduces the oxidizability of the slag and reduces the secondary oxidation of the slag to the molten steel. The recovery rate of Fe in the slag is increased and the iron loss is reduced. The low oxygen condition increases the alloy recovery rate and reduces the alloy oxidation consumption. The good kinetic conditions are conducive to the efficient floating of inclusions in the molten steel. The cleanliness of the molten steel is significantly improved, which is conducive to the improvement of the mechanical properties of the steel and the lightweight of the automobile.
[0056] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A production process for high-cleanliness ultra-low carbon steel, characterized in that: Through RH+VOD dual control, the molten steel is sent into the VOD furnace after RH decarburization treatment. After VOD reaches the vacuum requirement, the top gun is lowered to the slag surface to blow hydrogen, and air is blown through the bottom air bricks. The bottom hydrogen is blown to deoxidize the molten steel, and the top slag is modified by blowing hydrogen on the slag surface. Alloying is carried out after breaking the air, and no deoxidized alloy is used in the process.
2. The production process of high-cleanliness ultra-low carbon steel according to claim 1, characterized in that: The production process specifically includes: KR pretreatment, converter smelting, RH, VOD, and continuous casting.
3. The production process of high-cleanliness ultra-low carbon steel according to claim 2, characterized in that: KR pretreatment is used for hot metal desulfurization, and the [S] content in the hot metal after treatment is required to be ≤50×10 -6 .
4. The production process of high-cleanliness ultra-low carbon steel according to claim 2, characterized in that: The scrap steel ratio of converter smelting is controlled to be ≤22%; the FeO content at the end of blowing is ≤25wt%; the converter end temperature is required to be controlled at 1690~1710℃, and the end [C] content is controlled at (320~480)×10 -6 , end point [P] content ≤ 90 × 10 -6 , end point [S] content ≤ 55 × 10 -6 , end point [O] content ≥480×10 -6 ; Steel is tapped using a carbon-free ladle; 0.8-3.5kg / t of steel is added 钢 of lime.
5. The production process of high-cleanliness ultra-low carbon steel according to claim 2, characterized in that: Drive the ladle car to the RH station and start vacuuming and circulation. Use a five-stage or four-stage vacuum pump to vacuum to 5-15kPa to maintain the vacuum degree. Lower the oxygen lance to start forced decarburization. The oxygen blowing intensity is 1200-4200NL / t. 钢 / min, oxygen blowing time is 5 to 18min; after decarburization, the third-stage pump, the second-stage pump, and the first-stage pump are started in sequence at intervals of 1min. After the first-stage pump is started, the vacuum degree of the vacuum chamber is maintained at ≤67Pa, and the vacuum degree is maintained for 5 to 20min for natural decarburization; after decarburization, the vacuum chamber is opened and the station is exited. The exit requirement is [C] content ≤15×10 -6 , the molten steel temperature is required to be 1662~1688℃.
6. The production process of high-cleanliness ultra-low carbon steel according to claim 5, characterized in that: After RH leaves the station, no top slag modifier is added and it is directly sent to the VOD station.
7. The production process of high-cleanliness ultra-low carbon steel according to claim 6, characterized in that: After entering the VOD station, the ladle is covered and vacuum treatment begins. When the vacuum degree reaches 1500-3500Pa, the top gun is placed above the slag surface and a hydrogen-inert gas mixture with a hydrogen ratio of 10-50% is sprayed. The spraying intensity is 1500-4500NL / t. 钢 / min, the blowing time is 8 to 20min; at the same time, a hydrogen-inert gas mixture with a hydrogen ratio of 10 to 50% is blown into the bottom through the bottom air bricks, and multiple bottom blowing holes can be selected for bottom blowing, with a total gas supply intensity of 1200 to 6000NL / t 钢 / min, the blowing time is 8 to 30min; when the blowing volume reaches 50%, the vacuum degree continues to be reduced. When the hydrogen blowing is finished, the vacuum degree of the vacuum chamber is adjusted to ≤67Pa. Bottom-blown air-permeable bricks are used to blow argon into the molten steel to assist in degassing. The total gas supply intensity is 1200 to 4500NL / t 钢 / min, the blowing time is 5 to 15min; VOD outbound requirements are that the molten steel temperature is between 1585 and 1630℃, and the molten steel [C] content is ≤15×10 -6 , [O] content ≤ 15×10 -6 , [P] content ≤ 90 × 10 -6 , [N] content ≤ 30 × 10 -6 , [H] content ≤ 3 × 10 -6 , [S] content ≤ 50 × 10 -6 .
8. The production process of high-cleanliness ultra-low carbon steel according to claim 7, characterized in that: The amount of alloy to be added is calculated based on the composition of the molten steel tapped by VOD. After the alloy is added, soft blowing is performed for 5 to 10 minutes to ensure uniform composition of the molten steel. After alloying, the temperature of the molten steel is required to be controlled at 1570 to 1595°C, and the [C] content in the molten steel is ≤15×10 -6 , [Si] content ≤ 55 × 10 -6 , [Mn] content is (900-1300)×10 -6 , [P] content ≤ 90 × 10 -6 , [S] content ≤ 50 × 10 -6 , [Ti] content ≤ 110×10 -6 , [Als] content ≤ 15×10 -6 , [O] content ≤ 15×10 -6 , [N] content ≤ 30 × 10 -6 , [H] content ≤ 3 × 10 -6 .
9. The production process of high-cleanliness ultra-low carbon steel according to claim 2, characterized in that: The continuous casting adopts protective casting measures to strictly prevent the secondary oxidation of molten steel and control the temperature of the tundish at 1554-1570℃; the crystallizer covering agent adopts ultra-low carbon covering agent, and the whole continuous casting process is carried out with protective casting, and the process requires oxygen addition of less than 3×10 -6 , nitrogen addition is less than 3×10 -6 .
Citation Information
Patent Citations
Process for applying hydrogen to deoxygenation of liquid steel
CN101603115A
Method for generating micro bubbles in molten steel
CN106086315A
Induction furnace and RH-OB duplex process
CN108774662A
Melting method for HIC (Hydrogen Induced Crack)-resistant pipeline steel
CN109161630A
Production method of high-cleanliness bearing steel
CN113981306A