Method for reducing zirconium content in cast high-temperature alloy return scrap
By sorting, sand blowing, vacuum induction smelting and electroslag remelting, the problem of excessive zirconium content in the high-temperature alloy return material is solved, and the zirconium content is significantly reduced and the regeneration and utilization of the high-temperature alloy return material is achieved. The rate has increased, avoiding the waste of strategic metal resources.
Patent Information
- Application Number
- CN202410980242.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
AI Technical Summary
The content of zirconium in the return material of high temperature alloy is too high and difficult to remove, resulting in a degradation of casting performance and a waste of strategic metal resources, limiting the recycling of the return material of high temperature alloy.
Using block-by-block sorting and classification, sand blowing treatment, vacuum induction smelting and electroslag remelting, the surface impurities are removed through hand-held XRF analysis and sand blasting machine, vacuum induction smelting and electroslag remelting are removed. Control the slag-based components to reduce the zirconium content.
It effectively reduces the zirconium content in the return material of high-temperature alloy, improves the regeneration utilization rate, removes oil stains, inclusions and impurities, improves the purity of the return material of cast high-temperature alloy, and reduces the waste of valuable strategic resources.
Smart Images

Figure CN118910429A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-temperature alloy smelting and high-temperature alloy return material recycling, and in particular to a method for reducing the zirconium content in high-temperature alloy return material for casting. Background Art
[0002] High-temperature alloys are widely used in the preparation of hot-end components of aircraft engines and gas turbines due to their excellent high-temperature comprehensive properties. At present, domestic high-quality high-temperature alloys for aircraft engines and gas turbines still rely on imports. A large number of core alloying elements such as nickel, cobalt, niobium, and rhenium in high-temperature alloys are scarce strategic resources of the country. my country has low natural resource reserves of these rare and precious elements and is highly dependent on foreign countries. The preparation process of high-temperature alloys is numerous and complex, and the effective utilization rate of materials is as low as 10-20%. The utilization rate of some complex parts is even lower than 10%, and the rest exist in the form of risers, runners, and scrap parts. The return materials generated in my country each year are as high as thousands of tons.
[0003] Since the castings undergo a high-temperature melting process during production, the alloy melt contacts and reacts with the crucible, core, shell, filter, etc. at high temperatures, resulting in the return material containing more inclusions and impurity elements than the new material. Among them, Zr, as a control element for most alloys, will continue to accumulate in the high-temperature alloy return material, and it is difficult to remove it by vacuum induction melting. An appropriate amount of Zr can effectively improve the casting performance and mechanical properties of equiaxed high-temperature alloys, while excessive Zr will cause problems such as cracks and insufficient pouring of castings, and reduce the mechanical properties of the alloy. Zr, as a content control element for directional and single-crystal alloys, will increase the hot cracking tendency of directional and single-crystal castings. Therefore, the content of Zr is required to be strictly controlled in directional and single-crystal alloys. The large accumulation of Zr in the return material of casting high-temperature alloys exceeds the upper limit of the content control, and it is also difficult to remove, which seriously hinders the same-level recycling of high-temperature alloy return materials with strict requirements on Zr content, especially the more expensive directional and single-crystal high-temperature alloys, resulting in serious waste of strategic metal resources and a substantial increase in manufacturing costs. Summary of the invention
[0004] The purpose of the present invention is to overcome and supplement the deficiencies in the prior art and to provide a method for reducing the zirconium content in the return material of a cast high-temperature alloy, strictly controlling the Zr oxide content in the slag system to a minimum level, while appropriately increasing alumina to inhibit the decomposition of the extremely small amount of zirconium oxide content.
[0005] The technical solution adopted by the present invention is:
[0006] A method for reducing the zirconium content in a cast high-temperature alloy return material, comprising the following steps:
[0007] Step S1. Pre-treatment: sorting and classifying the returned high-temperature alloy materials piece by piece, performing sandblasting on the classified alloys, and finally purging the surface of the returned materials;
[0008] Step S2. Vacuum induction melting: subjecting the returned material after pretreatment to vacuum induction melting and refining, and then casting to obtain a vacuum induction ingot;
[0009] Step S3. electroslag remelting: polish the surface of the vacuum induction ingot to use it as an electroslag remelting electrode, and then electroslag remelt the electroslag remelting electrode under a protective atmosphere to obtain a processed casting high-temperature alloy return material.
[0010] Preferably, the method for reducing the zirconium content in the return material of the cast high-temperature alloy is as follows: in step S1, the return material of the cast high-temperature alloy is sorted and classified using a handheld XRF analyzer; the sand blasting treatment uses a sand blasting machine to perform surface sand blasting, the sand blasting pressure is 0.5-1MPa, and the sand blasting time is 15-30s; compressed air is used to purge the surface of the return material, and the purge time is 5-20s.
[0011] Preferably, the method for reducing the zirconium content in the return material of the cast high-temperature alloy, wherein: the vacuum degree during vacuum induction melting in step S2 is 0.055±0.045Pa, and the melting time is 4-10h; the refining temperature is 1500-1600℃, the number of refining times is 1-3 times, the time of each refining is 30-60min, and the pouring temperature is 1400-1600℃.
[0012] Preferably, in the method for reducing the zirconium content in the return material of the cast high-temperature alloy, the slag system of the electroslag remelting in step S3 includes 64%-65% CaF2, 15%-16% CaO, 1% MgO and 18%-19% Al2O3.
[0013] Preferably, in the method for reducing the zirconium content in the cast high-temperature alloy return material, the zirconium content of the cast high-temperature alloy return material after treatment in step S3 is reduced by 10-60%, and the sulfur content is reduced to less than 2 ppm.
[0014] Advantages of the present invention:
[0015] The method of reducing the zirconium content in the cast high-temperature alloy return material of the present invention reduces the zirconium content in the cast high-temperature alloy return material to 10-60%, effectively solves the problem that the zirconium element cannot be removed by vacuum induction melting alone, and improves the same-level recycling rate of the cast high-temperature alloy return material; at the same time, the return material pretreatment and vacuum induction melting are coordinated to effectively remove the outer surface oil and inclusions, internal gas, impurity elements and inclusions of the return material, thereby improving the purity of the cast high-temperature alloy return material alloy ingot, and greatly reducing the waste of precious strategic resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 The present invention is a flow chart of the method for reducing the zirconium content in the returned material of the casting high-temperature alloy. DETAILED DESCRIPTION
[0017] The present invention will be further described below in conjunction with specific embodiments.
[0018] Example 1
[0019] like Figure 1 A method for reducing the zirconium content in a cast high-temperature alloy IN792 return material comprises the following steps:
[0020] Step S1. Pretreatment: The cast high-temperature alloy IN792 return material (batch 1) is sorted and classified piece by piece using a handheld XRF analyzer, and the classified alloy is sandblasted using a sandblasting machine with a sandblasting pressure of 0.6 MPa and a sandblasting time of 30 seconds. Finally, the surface of the return material is purged with compressed air for 10 seconds;
[0021] Step S2. Vacuum induction melting: The returned material after purging in step S1 is subjected to vacuum induction melting and refining under a vacuum condition of 0.055±0.045Pa, and the melting time is 6h; the refining temperature is 1580°C, the refining number is 1, the refining time is 40min, and the vacuum induction ingot is cast at a casting temperature of 1500°C;
[0022] Step S3. electroslag remelting: polish the surface of the vacuum induction ingot as an electroslag remelting electrode, and then electroslag remelt the electroslag remelting electrode in an argon protective atmosphere. The slag system of the electroslag remelting contains CaF265wt%, CaO15wt%, MgO1wt%, and Al2O319wt%, and the zirconium oxide content in the slag system is strictly controlled to obtain the processed casting high-temperature alloy return material.
[0023] The changes in zirconium and sulfur contents in the cast high-temperature alloy return material after treatment in Example 1 are shown in Table 1.
[0024] Table 1 Changes in Zr and S content in alloy IN792 return material (batch 1)
[0025] Element Category Zr S Content of each element in the return material of cast high temperature alloy IN792 0.033wt% 0.0006wt% Content of each element in vacuum induction ingot 0.034wt% 0.0004wt% Content of each element in the returned material of casting high temperature alloy 0.019wt% 0.00018wt% Removal rate of each element 42.42% 70.00%
[0026] Example 2
[0027] like Figure 1 A method for reducing the zirconium content in a cast high-temperature alloy IN792 return material comprises the following steps:
[0028] Step S1. Pretreatment: The cast high-temperature alloy IN792 return material (batch 2) is sorted and classified piece by piece using a handheld XRF analyzer to ensure that there is no mixed grade alloy. The classified alloy is sandblasted using a sandblasting machine with a sandblasting pressure of 0.7 MPa and a sandblasting time of 25 seconds. Finally, the surface of the return material is purged with compressed air for 15 seconds.
[0029] Step S2. Vacuum induction melting: The returned material after purging in step S1 is subjected to vacuum induction melting and refining under a vacuum condition of 0.055±0.045Pa, and the melting time is 7h; the refining temperature is 1580°C, the refining times are 2 times, and the refining time for each time is 45min, and the vacuum induction ingot is cast, and the casting temperature is 1490°C;
[0030] Step S3. electroslag remelting: polish the surface of the vacuum induction ingot as an electroslag remelting electrode, and then electroslag remelt the electroslag remelting electrode in an argon protective atmosphere. The slag system of the electroslag remelting contains CaF264wt%, CaO16wt%, MgO1wt%, and Al2O319wt%, and the zirconium oxide content in the slag system is strictly controlled to obtain the processed casting high-temperature alloy return material.
[0031] The changes in zirconium and sulfur contents in the cast high-temperature alloy return material after treatment in Example 2 are shown in Table 2.
[0032] Table 2 Changes in Zr and S content in alloy IN792 return material (batch 2)
[0033] Element Category Zr S Content of each element in the return material of cast high temperature alloy IN792 0.030wt% 0.0005wt% Content of each element in vacuum induction ingot 0.029wt% 0.00034wt% Content of each element in the returned material of casting high temperature alloy 0.018wt% 0.00008wt% Removal rate of each element 40.00% 84.00%
[0034] Example 3
[0035] like Figure 1 A method for reducing the zirconium content in a cast high-temperature alloy IN792 return material comprises the following steps:
[0036] Step S1. Pretreatment: The cast high-temperature alloy IN792 return material (batch 3) is sorted and classified piece by piece using a handheld XRF analyzer to ensure that there is no mixed grade alloy. The classified alloy is sandblasted using a sandblasting machine with a sandblasting pressure of 0.7 MPa and a sandblasting time of 30 seconds. Finally, the surface of the return material is purged with compressed air for 20 seconds.
[0037] Step S2. Vacuum induction melting: The returned material after purging in step S1 is subjected to vacuum induction melting and refining under a vacuum condition of 0.055±0.045Pa, and the melting time is 8h; the refining temperature is 1590°C, the refining times are 3 times, and the refining time for each time is 30min, and the vacuum induction ingot is cast, and the casting temperature is 1490°C;
[0038] Step S3. electroslag remelting: polish the surface of the vacuum induction ingot as an electroslag remelting electrode, and then electroslag remelt the electroslag remelting electrode in an argon protective atmosphere. The slag system of the electroslag remelting contains CaF265wt%, CaO16wt%, MgO1wt%, and Al2O318wt%, and the zirconium oxide content in the slag system is strictly controlled to obtain the processed casting high-temperature alloy return material.
[0039] The changes in zirconium and sulfur contents in the cast high-temperature alloy return material after treatment in Example 3 are shown in Table 3.
[0040] Table 3 Changes in Zr and S content in alloy IN792 return material (batch 3)
[0041] Element Category Zr S Content of each element in the return material of cast high temperature alloy IN792 0.029wt% 0.0005wt% Content of each element in vacuum induction ingot 0.029wt% 0.0003wt% Content of each element in the returned material of casting high temperature alloy 0.020wt% 0.00009wt% Removal rate of each element 31.03% 82.00%
[0042] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for reducing the zirconium content in a cast high-temperature alloy return material, characterized in that: The following steps are involved: Step S1. Pre-treatment: sorting and classifying the returned high-temperature alloy materials piece by piece, sandblasting the classified alloys, and finally purging the surface of the returned materials; Step S2. Vacuum induction melting: vacuum induction melting and refining the returned material after pretreatment, and then casting to obtain a vacuum induction ingot; Step S3. Electroslag remelting: The vacuum induction ingot is surface-polished to serve as an electroslag remelting electrode, and then the electroslag remelting electrode is electroslag remelted under a protective atmosphere to obtain a processed casting high-temperature alloy return material.
2. The method for reducing the zirconium content in the returned material of the casting high-temperature alloy according to claim 1, characterized in that: In step S1, a handheld XRF analyzer is used for sorting and classification of the returned material of the cast high-temperature alloy; a sandblasting machine is used for surface sandblasting with a sandblasting pressure of 0.5-1MPa and a sandblasting time of 15-30s; compressed air is used to purge the surface of the returned material for 5-20s.
3. The method for reducing the zirconium content in the returned material of the casting high-temperature alloy according to claim 1, characterized in that: The vacuum degree during vacuum induction melting in step S2 is 0.055±0.045Pa, and the melting time is 4-10h; the refining temperature is 1500-1600°C, the number of refining times is 1-3 times, the time of each refining is 30-60min, and the pouring temperature is 1400-1600°C.
4. The method for reducing the zirconium content in the returned material of the casting high temperature alloy according to claim 1, characterized in that: In terms of mass percentage, the slag system of the electroslag remelting in step S3 includes 64%-65% CaF2, 15%-16% CaO, 1% MgO and 18%-19% Al2O3.
5. The method for reducing the zirconium content in the returned material of the casting high-temperature alloy according to claim 1, characterized in that: The zirconium content of the cast high-temperature alloy return material after treatment in step S3 is reduced by 10-60%, and the sulfur content is reduced to less than 2 ppm.