Purification method of high-purity tantalum
Through the combination of chlorination reaction, extraction, distillation and reduction reaction, the existing tantalum purification methods are solved, with high energy consumption and low efficiency, and efficient purification of high-purity tantalum is achieved to meet the needs of high-end applications.
Patent Information
- Application Number
- CN202410980493.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
AI Technical Summary
The existing tantalum purification methods are complex in operation, high energy consumption and low purification efficiency, making it difficult to meet the needs of high-purity materials.
The purity of tantalum chloride is improved by reacting with dry chlorine by combining chlorine, followed by extraction agent and distillation treatment, and the purity of tantalum is improved by aluminum thermal reduction or vacuum carbon reduction. Finally, high purity is achieved by pickling and drying.
The purification of high-purity tantalum is achieved, with a purity of more than 99.999%, reducing energy consumption and production costs, simplifying the operating process, and improving purification efficiency.
Smart Images

Figure CN118910431A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal element preparation, and in particular to a method for purifying high-purity tantalum. Background Art
[0002] In the metal processing and semiconductor material industries, high-purity tantalum (niobium / molybdenum / tungsten) materials have broad application prospects, especially in the manufacture of capacitors, electrodes, optical devices and semiconductor devices. However, since these metals usually exist in the form of low-purity ores in nature, a series of complex purification processes are required to obtain high-purity products.
[0003] In the prior art, traditional purification methods include electrolysis, zone smelting, etc., but these methods usually have problems such as complex operation, high energy consumption, and low purification efficiency.
[0004] Therefore, we need a method for purifying high-purity tantalum to solve the problems of complex operation, high energy consumption, and low purification efficiency of existing purification methods; it can achieve simple operation, high purification efficiency, and low energy consumption. Summary of the invention
[0005] The purpose of the present invention is to provide a method for purifying high-purity tantalum to solve the problems of complex operation, high energy consumption, low purification efficiency, etc. of the existing purification methods proposed in the above background technology; it can achieve simple operation, high purification efficiency and low energy consumption.
[0006] To achieve the above object, the present invention provides the following technical solution: a method for purifying high-purity tantalum, the method comprising the following steps:
[0007] Preparation of raw materials for purification of high purity tantalum;
[0008] Carrying out chlorination reaction on the prepared raw materials;
[0009] Separation and purification of raw materials after chlorination reaction;
[0010] Reduction reaction;
[0011] The raw material obtained after the reduction reaction is post-treated.
[0012] Preferably, the specific operations of preparing raw materials for purification of high-purity tantalum include:
[0013] Tantalum with a purity of at least 99.9% is selected as a raw material, and the mass of the raw material is 100 grams;
[0014] Prepare to use a mechanical crusher to crush the raw material to a particle size between 60 and 80 meshes, and use tantalum powder as the raw material powder to obtain a uniformly distributed raw material powder.
[0015] Preferably, the specific operation of chlorination reaction of the prepared raw materials includes:
[0016] Prepare a 1-liter reaction container and ensure that the inner wall of the container is clean and free of impurities;
[0017] Gently pour the crushed raw material powder into the reaction kettle container, and install the gas inlet and outlet and stirring device; the waste chlorine recovery system after drying adopts the existing system: condensation in condenser - reuse in reflux recovery tank, tail gas alkaline water spray circulation absorption - activated carbon adsorption neutralization - standard discharge;
[0018] Set the reaction temperature to 550°C and turn on the heating device at a heating rate of 10°C per minute;
[0019] When the temperature reaches 550°C, the dried chlorine gas is introduced. The flow rate of the dried chlorine gas is set to 10 liters per hour and the continuous introduction time is 6 hours.
[0020] While introducing the dried chlorine gas, turn on the stirring device and set the stirring speed to 100 revolutions per minute to ensure that the raw materials are fully in contact with the dried chlorine gas;
[0021] After the chlorination reaction continued for 6 hours, the dried chlorine gas supply and the stirring device were turned off, and the dried chlorine gas in the reactor was replaced with argon gas, and then the reaction vessel was allowed to cool naturally to room temperature.
[0022] Preferably, the specific operation of separating and purifying the raw materials after the chlorination reaction includes:
[0023] The gas in the reaction vessel is discharged and the tantalum chloride therein is collected, the mass of the chloride being 80 g;
[0024] Dissolve the chloride in 500 ml of carbon tetrachloride to obtain a uniform solution;
[0025] The solution was extracted with dichloromethane as an extractant, the amount of the extractant was 300 ml, and the number of extractions was 3 times;
[0026] The extracted solution was distilled at a temperature of 100° C. for 2 hours.
[0027] The pure tantalum chloride obtained after distillation was collected, with a mass of 75 grams;
[0028] The purity of chloride should be above 99.99%.
[0029] Preferably, the specific operation of the reduction reaction includes:
[0030] High-purity tantalum is obtained by aluminothermic reduction or vacuum carbon reduction.
[0031] Preferably, the specific operation of post-processing the raw material obtained after the reduction reaction includes:
[0032] The reduced metal is pickled using 10% hydrochloric acid for 30 minutes;
[0033] After pickling, use clean water to wash the metal several times with pure water and filter it until it is neutral;
[0034] Put the washed metal into the drying oven, set the drying temperature to 80-100℃ and the drying time to 2 hours;
[0035] The purity of the dried metal is tested and the purity should reach above 99.999%.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] The high-purity tantalum purification method proposed in the present invention can effectively remove impurities in the raw materials through chlorination reaction and subsequent reduction, distillation and other steps, thereby obtaining high-purity tantalum (niobium / molybdenum / tungsten) products with a purity of more than 99.999%, meeting the needs of high-end application fields; by accurately controlling the reaction conditions, energy consumption can be reduced and energy utilization efficiency can be improved. This is not only conducive to reducing production costs, but also conducive to environmental protection; it further solves the problems of complex operation, high energy consumption, and low purification efficiency of existing purification methods; it can achieve simple operation, high purification efficiency, and low energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 The figure is a flow chart of the method of the present invention. DETAILED DESCRIPTION
[0039] In order to make the purpose and technical solution of the present invention clearly and completely described, and the advantages more clearly understood, the embodiments of the present invention are further described in detail with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are part of the embodiments of the present invention, rather than all of the embodiments, and are only used to explain the embodiments of the present invention, and are not used to limit the embodiments of the present invention. All other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] For example, see Figure 1 The present invention provides a technical solution: a method for purifying high-purity tantalum, the method comprising the following steps:
[0041] 1. Raw material preparation for high purity tantalum purification:
[0042] 1. Raw material selection
[0043] Raw material purity: Tantalum with a purity of at least 99.9% is selected as raw material to ensure a high starting purity, which helps the subsequent purification process to proceed smoothly.
[0044] Raw material mass: The mass of the raw material is set at 100 grams. This is to carry out standardized experimental operations and facilitate material calculation and proportioning in subsequent steps.
[0045] 2. Raw material crushing
[0046] Mechanical crusher selection: According to the hardness and quantity of the raw materials, choose a suitable mechanical crusher for crushing. The model and specification of the crusher should meet the requirements of crushing to the specified particle size.
[0047] Crushing operation: Put the raw materials into the crusher and crush them according to the equipment operating instructions. During the crushing process, attention should be paid to controlling the speed and crushing time of the crusher to ensure that the raw materials are crushed evenly and the particle size meets the requirements.
[0048] Particle size control: After crushing, the raw material is checked for particle size. The raw material powder with a particle size between 60 and 80 mesh is screened out through tools such as sieves. This part of the powder will be used as the raw material for the subsequent purification process.
[0049] 3. Raw material pretreatment
[0050] Cleaning: Clean the crushed raw material powder to remove impurities and dust. Deionized water or solvents such as ethanol can be used for cleaning.
[0051] Drying: The cleaned raw material powder needs to be dried to remove moisture. The drying temperature and time should be selected according to the characteristics of the raw materials and equipment conditions.
[0052] 2. Carry out chlorination reaction on the prepared raw materials:
[0053] 1. Preparation of reaction vessel
[0054] Choose an appropriate reaction vessel: Select a 1-liter, high-temperature, corrosion-resistant reaction vessel to ensure that the container can withstand high temperatures and the corrosion of dried chlorine gas.
[0055] Clean the reaction vessel: Use appropriate cleaning agents (such as deionized water, alcohol, etc.) and tools (such as brushes, cloths, etc.) to thoroughly clean the inner wall of the reaction vessel to ensure that there is no dust, oil or other impurities.
[0056] Dry container: Dry the cleaned container. You can use a hot air gun, drying oven and other equipment to ensure that the inner wall of the container is completely dry.
[0057] 2. Raw material delivery and equipment installation
[0058] Evenly place raw materials: Place the crushed raw material powder evenly into the reaction container to avoid local accumulation or uneven density.
[0059] Install gas inlet and outlet: Install the gas inlet and outlet on the reaction vessel to ensure that the dried chlorine gas can enter and discharge the container smoothly.
[0060] Install the stirring device: According to the structure and size of the reaction vessel, select a suitable stirring device (such as a stirring paddle, agitator, etc.) and install it correctly on the reaction vessel.
[0061] 3. Heating and chlorine
[0062] Set the reaction temperature: According to the experimental requirements, set the reaction temperature to 550°C. Ensure that the heating equipment can provide the required heat stably and evenly.
[0063] Heating process: Turn on the heating device and gradually increase the temperature in the reaction vessel at a heating rate of 10°C per minute. During the heating process, pay close attention to the temperature changes to ensure that the temperature is controlled within the set range.
[0064] Feed dried chlorine: When the temperature reaches 550°C, start feeding dried chlorine. Ensure that the flow rate of dried chlorine is set to 10 liters per hour and use a flow meter for real-time monitoring. The time for feeding dried chlorine should be set to 6 hours to ensure that the raw materials and dried chlorine react fully.
[0065] 4. Stirring and mixing
[0066] Turn on the stirring device: Turn on the stirring device while introducing the dried chlorine gas. Set the stirring speed to 100 revolutions per minute to ensure that the raw materials are evenly distributed in the reaction vessel and fully contacted with the dried chlorine gas.
[0067] Monitoring of the stirring process: During the stirring process, pay close attention to the stirring effect to ensure that the raw materials and the dried chlorine are evenly mixed. If necessary, adjust the stirring speed or stirring method in time.
[0068] 5. Cooling and post-processing
[0069] Shut down the dried chlorine supply and stirring device: After the chlorination reaction lasts for 6 hours, shut down the dried chlorine supply and stirring device. Ensure that all operations are carried out in accordance with safety regulations to avoid leakage or accidents of dried chlorine.
[0070] Natural cooling: Allow the reaction vessel to cool naturally to room temperature. During the cooling process, avoid violent vibration or impact on the container to avoid adverse effects on the reaction products.
[0071] 3. Separate and purify the raw materials after chlorination reaction:
[0072] 1. Gas export and chloride collection
[0073] Gas outlet: After the chlorination reaction is completed, first turn off the dried chlorine supply and ensure that the gas in the reaction vessel is safely discharged. This can be done by opening the gas outlet valve and using an appropriate collection device (such as a gas collection bag or a gas absorption device) to collect any remaining dried chlorine.
[0074] Chloride collection: After the gas in the reaction vessel is completely discharged, open the reaction vessel and carefully collect the tantalum chloride in it. Since tantalum chloride is a solid, it can be scraped off the inner wall and bottom of the container with a scraper or similar tool and collected in a dry, clean container. Ensure that the mass of the collected tantalum chloride is accurate and record it as 80 grams.
[0075] 2. Chloride dissolution
[0076] Solvent preparation: Prepare 500 ml of carbon tetrachloride as solvent. Make sure the quality of carbon tetrachloride meets the experimental requirements and the container is clean and free of impurities.
[0077] Dissolution operation: slowly add the collected tantalum chloride into carbon tetrachloride and stir with a stirrer or magnetic stirrer to promote the dissolution of tantalum chloride. During the stirring process, pay attention to the color and uniformity of the solution to ensure that the tantalum chloride is completely dissolved in carbon tetrachloride.
[0078] 3. Extraction operation
[0079] Extraction solvent preparation: Prepare 300 ml of dichloromethane as the extraction solvent. Make sure the quality of dichloromethane meets the experimental requirements and the container is clean and free of impurities.
[0080] Extraction process: Pour the carbon tetrachloride solution containing tantalum chloride into a separatory funnel, and then slowly add dichloromethane. During the addition process, gently shake the separatory funnel to promote mixing between the two solutions. Wait for a while to allow the two solutions to fully separate. Then, open the bottom valve of the separatory funnel, release the dichloromethane solution containing tantalum chloride in the lower layer, and collect it in another container. Repeat this operation 3 times to ensure that the tantalum chloride is fully extracted.
[0081] 4. Distillation
[0082] Distillation equipment preparation: Prepare appropriate distillation equipment, including distillation flask, condenser, receiving bottle, etc. Make sure the equipment is clean, free of impurities, and the connections are tight and leak-free.
[0083] Distillation operation: Pour the dichloromethane solution containing tantalum chloride obtained after extraction into the distillation flask, and install the condenser and receiving bottle. Then, turn on the heating equipment, set the distillation temperature to 100℃, and start distillation. During the distillation process, pay attention to the liquid volume and temperature changes in the receiving bottle to ensure that the distillation process is stable. The distillation time is 2 hours to ensure that most of the dichloromethane is evaporated and pure tantalum chloride is left.
[0084] 5. Chloride collection and purity testing
[0085] Chloride collection: After the distillation is completed, turn off the heating equipment and wait for the liquid in the receiving bottle to cool to room temperature. Then, carefully collect the pure tantalum chloride in the receiving bottle and record its mass as 75 grams.
[0086] Purity test: The collected tantalum chloride is tested for purity. Spectroscopic analysis, chemical analysis or other appropriate methods can be used for testing. The purity should be above 99.99% to ensure the quality requirements of subsequent experiments or applications. If the purity does not meet the requirements, re-purification or other appropriate treatments can be considered.
[0087] 4. Specific operation of reduction reaction:
[0088] High-purity tantalum is obtained by aluminothermic reduction or vacuum carbon reduction. For the aluminothermic reduction method, the aluminothermic reduced material is directly cleaned of aluminum slag after being taken out of the furnace, broken into pieces, and then smelted in a horizontal electron beam furnace for the first time to remove aluminum (a layer of main metal powder is laid on the bottom) to avoid the electron beam from sweeping through the furnace body and crucible, and made into a plate shape, and then cut into strips by a shearing machine, and tied into rods, and then smelted into ingots in a vertical electron beam furnace for the second time to increase purity, and smelted twice.
[0089] 5. Specific operation of post-processing the raw materials obtained after the reduction reaction:
[0090] 1. Pickling treatment
[0091] Pickling solution preparation: Prepare a 10% hydrochloric acid solution. Make sure the quality of the hydrochloric acid meets the experimental requirements and the container is clean and free of impurities. The volume of the hydrochloric acid solution should be determined according to the size and surface area of the metal block to ensure that the metal can be completely immersed in the pickling solution.
[0092] Pickling operation: Carefully place the reduced metal into the pickling solution, ensuring that the metal is completely immersed in the solution. Turn on the stirring device (if available) to promote full contact between the metal and the pickling solution. The pickling time is 30 minutes, during which time the changes in the metal surface should be closely monitored to ensure uniform pickling effect.
[0093] Observation after pickling: After pickling, take the metal out of the pickling solution and observe whether the metal surface is clean and free of residue. If necessary, use a soft brush to gently scrub the metal surface to remove stubborn residues.
[0094] 2. Rinse
[0095] Pure water preparation: Prepare enough pure water for rinsing the metal. Make sure the pure water temperature is moderate to avoid thermal shock to the metal.
[0096] Rinsing operation: Rinse the pickled metal in clean water. During the rinsing process, flowing clean water should be used to ensure that the pickling solution on the metal surface is completely rinsed. The rinsing time should be long enough until the rinse solution is neutral and can be tested with pH test paper.
[0097] Observation after rinsing: After rinsing, take the metal out of the clean water and observe whether the metal surface is clean and free of water droplets. If necessary, you can use a clean cloth or paper towel to gently wipe the metal surface to remove residual moisture.
[0098] 3. Drying
[0099] Drying box preparation: Prepare the drying box appropriately, making sure the interior of the drying box is clean and free of impurities, and that the heating elements and temperature control system are working properly.
[0100] Placing the metal: Place the washed metal in the drying oven, making sure the metal is evenly distributed in the drying oven so that it is heated evenly.
[0101] Set drying parameters: Set the drying temperature to 80-100℃ and the drying time to 2 hours. These parameters should be adjusted according to the type and size of the metal to ensure that the metal can be completely dried.
[0102] Start drying: Turn on the drying oven and dry according to the set drying parameters. During the drying process, pay close attention to the temperature changes in the drying oven to ensure that the temperature is controlled within the set range.
[0103] Observation after drying: After drying, close the drying oven and wait for the metal to cool down to room temperature naturally. Then take out the metal and observe whether the metal surface is dry and free of moisture.
[0104] 4. Purity testing
[0105] Purity detection method selection: Select the appropriate purity detection method according to the type of metal and purity requirements. Commonly used purity detection methods include spectral analysis, chemical analysis, X-ray diffraction, etc.
[0106] Purity test operation: Perform purity test according to the operating instructions of the selected purity test method. During the test, the representativeness and accuracy of the sample should be ensured to obtain accurate purity results.
[0107] Purity result analysis: Based on the purity test results, analyze whether the purity of the metal meets the requirements (99.999% or more). If the purity does not meet the requirements, re-purification or other appropriate treatment can be considered.
[0108] Example 2, based on Example 1, proposes a method for purifying high-purity tantalum by chlorination:
[0109] 1. Raw material preparation
[0110] Tantalum raw material with a purity of 99.9% and a mass of 100 grams was selected.
[0111] Put the raw materials into the crusher and crush them into a particle size range of 60 to 80 mesh.
[0112] 2. Chlorination reaction
[0113] Prepare a 1-liter high-temperature resistant glass reaction container and ensure that the inner wall of the container is clean and free of impurities.
[0114] Place the crushed tantalum raw material evenly into the reaction container, and install the gas inlet and outlet and stirring device.
[0115] The reaction temperature was set to 550°C, and the heating device was turned on to heat to the target temperature at a rate of 10°C per minute.
[0116] When the temperature reaches 550°C, the dried chlorine gas is introduced. The flow rate of the dried chlorine gas is set at 10 liters per hour and the introduction is continued for 6 hours.
[0117] While introducing the dried chlorine gas, the stirring device was turned on and the stirring speed was set to 100 revolutions per minute to ensure that the raw materials were fully in contact with the dried chlorine gas.
[0118] 3. Separation and purification
[0119] After the chlorination reaction is completed, the dried chlorine gas supply and the stirring device are turned off, and the reaction vessel is allowed to cool naturally to room temperature.
[0120] Tantalum chloride was collected in the reaction vessel, with a mass of 85 g.
[0121] Tantalum chloride is dissolved in 500 ml of carbon tetrachloride to obtain a tantalum chloride solution.
[0122] The tantalum chloride solution was extracted using dichloromethane as an extractant, 300 ml of the extractant was used each time, and the extraction was performed three times.
[0123] The extracted solution was distilled at a temperature of 100° C. for 2 hours to obtain pure tantalum chloride with a mass of 78 grams.
[0124] 4. Reduction reaction
[0125] Pure tantalum chloride and metallic sodium are mixed evenly in a molar ratio of 1:1.2.
[0126] Under argon protection, the mixture was placed in a tube furnace and the heating temperature was set to 700 °C.
[0127] The temperature was heated to the target temperature at a rate of 15°C per minute and maintained for 3 hours for the reduction reaction.
[0128] 5. Post-processing
[0129] After the reduction reaction was completed, the heating device was turned off and the mixture was allowed to cool naturally to room temperature.
[0130] The reduced tantalum was pickled using hydrochloric acid with a concentration of 10% for 30 minutes.
[0131] After pickling, the tantalum is washed with deionized water several times and filtered to neutrality.
[0132] The rinsed tantalum was placed in a drying oven, and the drying temperature was set to 80-100°C and the drying time was set to 2 hours.
[0133] The purity of the dried tantalum is tested and the purity should be above 99.999%.
[0134] It should be noted that, when preparing high-purity tantalum in this embodiment, the niobium content in tantalum is the focus of extraction and separation, and the extraction and separation of niobium may be achieved by the following methods:
[0135] Chlorination stage: In the chlorination reaction, the tantalum raw material reacts with the dried chlorine gas to form tantalum chloride (TaCl 5 ), and niobium (if present) will also react with the dried chlorine to form the corresponding chloride (such as NbCl 5 ). The behavior of these chlorides in subsequent processing may vary, but they will generally dissolve in the solvent.
[0136] Solvent extraction: After dissolving tantalum chloride in carbon tetrachloride, the extraction is performed using dichloromethane or other extractants. Due to the difference in solubility of different chlorides in the solvent, a certain degree of separation can be achieved. Although the main purpose of this step is to purify tantalum chloride, it will also indirectly reduce the content of impurities including niobium.
[0137] Distillation treatment: During the distillation process, different chlorides will be distilled at different temperatures due to their different boiling points. By controlling the distillation temperature and time, low-boiling or high-boiling impurities including niobium chloride can be further removed.
[0138] Selective reduction: In the reduction reaction stage, although the main purpose is to reduce tantalum chloride to metallic tantalum, the reducing agent (such as metallic sodium) may have different reduction activities for different chlorides. If the reduction activity of niobium chloride is low, then the niobium content may be further reduced in this step.
[0139] Post-treatment: Pickling and rinsing steps are primarily used to remove residues and impurities from the surface of the reduced product, including niobium that may be present in the form of oxides or other forms.
[0140] Example 3, based on Example 1, proposes a method for purifying high-purity niobium by chlorination:
[0141] 1. Raw material preparation
[0142] A niobium raw material with a purity of 99.8% and a mass of 150 grams was selected.
[0143] Put the raw materials into the crusher and crush them into a particle size range of 40 to 60 mesh.
[0144] 2. Chlorination reaction
[0145] Prepare a 2-liter high-temperature quartz reaction container and ensure that the inner wall of the container is clean and free of impurities.
[0146] The crushed niobium raw materials are evenly placed in the reaction vessel, and the gas inlet and outlet and stirring device are installed.
[0147] The reaction temperature was set to 600°C, and the heating device was turned on to heat to the target temperature at a rate of 15°C per minute.
[0148] When the temperature reaches 600°C, the dried chlorine gas is introduced. The flow rate of the dried chlorine gas is set to 15 liters per hour and the introduction is continued for 8 hours.
[0149] While introducing the dried chlorine gas, the stirring device was turned on and the stirring speed was set to 150 revolutions per minute to ensure that the raw materials were fully in contact with the dried chlorine gas.
[0150] 3. Separation and purification
[0151] After the chlorination reaction is completed, the dried chlorine gas supply and the stirring device are turned off, and the reaction vessel is allowed to cool naturally to room temperature.
[0152] The niobium chloride in the reaction vessel was collected, with a mass of 130 g.
[0153] Niobium chloride was dissolved in 600 ml of benzene to obtain a niobium chloride solution.
[0154] The niobium chloride solution was extracted using toluene as an extractant, 400 ml of the extractant was used each time, and the extraction was performed 4 times.
[0155] The extracted solution was distilled at a temperature of 120° C. for 3 hours to obtain pure niobium chloride with a mass of 120 g.
[0156] 4. Reduction reaction
[0157] Pure niobium chloride and metallic magnesium were mixed uniformly at a molar ratio of 1:1.5.
[0158] Under argon protection, the mixture was placed in a tube furnace and the heating temperature was set to 800 °C.
[0159] The temperature was heated at a rate of 20°C per minute to the target temperature and maintained for 4 hours for the reduction reaction.
[0160] 5. Post-processing
[0161] After the reduction reaction is completed, turn off the heating equipment and let the mixture cool naturally to room temperature. This process requires patience to ensure that the reaction is completed safely and to avoid danger or impact on product purity due to sudden cooling.
[0162] When the mixture is completely cooled, open the reaction vessel and take out the reduced tungsten. At this point, the tungsten may still contain some unreacted impurities or residues, which require further cleaning.
[0163] The reduced tungsten is pickled with 10% hydrochloric acid for 1 hour. This step is to remove possible oxides or other impurities.
[0164] After pickling, the tungsten is rinsed several times with deionized water until the rinse solution is neutral to ensure that all residual acid and impurities are removed.
[0165] Put the rinsed tungsten into the drying oven, set the drying temperature to 80-100℃ and the drying time to 4 hours. The purpose of drying is to remove moisture and prevent the product from rusting or deterioration.
[0166] The purity of the dried tungsten is tested. The purity test can be carried out by spectral analysis, chemical analysis or other appropriate methods. The purity should meet the predetermined standard, such as above 99.999%;
[0167] The solution of this embodiment can also be used to purify niobium. The purity of the purified niobium should reach above 99.999%.
[0168] It should be noted that, when preparing high-purity niobium in this embodiment, the tantalum content in niobium is the focus of extraction and separation, and the difference in solubility of tantalum and niobium in certain solvents is used for separation:
[0169] The niobium chloride solution obtained after the chlorination reaction (which may contain some tantalum chloride) is mixed with a solvent having a higher selectivity for tantalum (such as some organic solvent or complex solution).
[0170] The solution is mixed thoroughly by stirring so that the tantalum chloride is preferentially transferred to the solvent phase.
[0171] The solvent phase and the aqueous phase or benzene phase containing niobium are separated, thereby achieving the preliminary separation of tantalum and niobium.
[0172] Embodiment 4, on the basis of embodiment 1, proposes a method for purifying high-purity molybdenum by chlorination method:
[0173] 1. Raw material preparation
[0174] A molybdenum raw material with a purity of 99.8% and a mass of 200 grams was selected.
[0175] Put the raw materials into a ball mill and grind them to a particle size range of 40 to 60 mesh.
[0176] 2. Chlorination reaction
[0177] Prepare a 2-liter high-temperature quartz reaction container and ensure that the inner wall of the container is clean and free of impurities.
[0178] Place the crushed molybdenum raw materials evenly into the reaction vessel, and install the gas inlet and outlet and stirring device.
[0179] The reaction temperature was set to 650°C, and the heating device was turned on to heat to the target temperature at a rate of 15°C per minute.
[0180] When the temperature reaches 650°C, the dried chlorine gas is introduced. The flow rate of the dried chlorine gas is set at 15 liters per hour and the introduction is continued for 8 hours.
[0181] While introducing the dried chlorine gas, the stirring device was turned on and the stirring speed was set to 150 revolutions per minute to ensure that the raw materials were fully in contact with the dried chlorine gas.
[0182] 3. Separation and purification
[0183] After the chlorination reaction is completed, the dried chlorine gas supply and the stirring device are turned off, and the reaction vessel is allowed to cool naturally to room temperature.
[0184] The molybdenum chloride in the reaction vessel was collected, with a mass of 180 g.
[0185] Molybdenum chloride was dissolved in 600 ml of carbon tetrachloride to obtain a molybdenum chloride solution.
[0186] The molybdenum chloride solution was extracted using dichloromethane as an extractant, 400 ml of the extractant was used each time, and the extraction was performed 4 times.
[0187] The extracted solution was distilled at 120°C for 3 hours to obtain pure molybdenum chloride with a mass of 170 g.
[0188] 4. Reduction reaction
[0189] Pure molybdenum chloride and metallic calcium were mixed evenly in a molar ratio of 1:1.8.
[0190] Under argon protection, the mixture was placed in a tube furnace and the heating temperature was set to 850 °C.
[0191] The temperature was heated to the target temperature at a rate of 20°C per minute and maintained for 5 hours for the reduction reaction.
[0192] 5. Post-processing
[0193] After the reduction reaction was completed, the heating device was turned off and the mixture was allowed to cool naturally to room temperature.
[0194] The reduced molybdenum was pickled using hydrochloric acid with a concentration of 10% for 40 minutes.
[0195] After pickling, the molybdenum is washed with pure water several times and filtered until it becomes neutral.
[0196] The rinsed molybdenum was placed in a drying oven, and the drying temperature was set to 100°C and the drying time was set to 3 hours.
[0197] The purity of the dried molybdenum should be tested and the purity should be above 99.999%;
[0198] Tungsten can also be purified by the solution of this embodiment, and the purity of the purified tungsten should reach more than 99.999%.
[0199] It should be noted that, when preparing high-purity molybdenum in this embodiment, the tungsten content in molybdenum is the focus of extraction and separation, and the specific operation of extraction and separation includes:
[0200] Chlorination reaction stage:
[0201] During the chlorination reaction, the reaction conditions (such as temperature, flow rate of dried chlorine gas, stirring speed) are optimized to promote the complete conversion of molybdenum and tungsten into the corresponding chlorides as much as possible. Since the selectivity and conditions of the chlorination reaction may vary, the proportion of the chlorinated products can be affected to a certain extent by fine-tuning the reaction conditions.
[0202] Extraction and separation stage:
[0203] Selective extraction: Use a solvent system with selective extraction ability in the molybdenum chloride solution, such as some organic solvents or ionic liquids. These solvents may have different solubility or complexing ability for molybdenum chloride and tungsten chloride. Through multiple extractions, most of the tungsten chloride can be separated from the solution.
[0204] Selection of extraction agent: Select the appropriate extraction agent based on the difference in solubility of molybdenum chloride and tungsten chloride in different solvents. For example, some solvents may have a stronger extraction ability for tungsten chloride, but a weaker extraction ability for molybdenum chloride.
[0205] Optimization of extraction conditions: By adjusting the concentration of the extractant, extraction temperature, extraction time and other conditions, the extraction effect can be optimized and the removal rate of tungsten impurities can be improved.
[0206] Subsequent processing:
[0207] After extraction and separation, the tungsten-containing extract is further treated, such as stripping or distillation, to recover the extractant and treat the tungsten impurities therein.
[0208] The extracted molybdenum chloride solution is subjected to subsequent purification steps, such as distillation, crystallization, etc., to further improve the purity of molybdenum.
[0209] Example 5, based on Example 1, proposes a method for purifying high-purity tungsten by chlorination:
[0210] 1. Raw material preparation
[0211] The tungsten raw material with a purity of 99.7% and a mass of 300 grams was selected.
[0212] Put the raw materials into the crusher and crush them into a particle size range of 30 to 50 mesh.
[0213] 2. Chlorination reaction
[0214] Prepare a 3-liter high-temperature resistant ceramic reaction container and ensure that the inner wall of the container is clean and free of impurities.
[0215] Place the crushed tungsten raw materials evenly into the reaction vessel, and install the gas inlet and outlet and stirring device.
[0216] The reaction temperature was set to 650°C, and the heating device was turned on to heat to the target temperature at a rate of 15°C per minute.
[0217] When the temperature reaches 650°C, the dried chlorine gas is introduced. The flow rate of the dried chlorine gas is set at 18 liters per hour and the introduction is continued for 9 hours.
[0218] While introducing the dried chlorine gas, the stirring device was turned on and the stirring speed was set to 180 revolutions per minute to ensure that the raw materials were fully in contact with the dried chlorine gas.
[0219] 3. Separation and purification
[0220] After the chlorination reaction is completed, the dried chlorine gas supply and the stirring device are turned off, and the reaction vessel is allowed to cool naturally to room temperature.
[0221] The tungsten chloride in the reaction vessel was collected, with a mass of 280 g.
[0222] Tungsten chloride was dissolved in 800 ml of toluene to obtain a tungsten chloride solution.
[0223] The tungsten chloride solution was extracted using xylene as an extractant, 500 ml of the extractant was used each time, and the extraction was performed 4 times.
[0224] The extracted solution was distilled at a temperature of 130° C. for 3 hours to obtain pure tungsten chloride with a mass of 260 g.
[0225] 4. Reduction reaction
[0226] Pure tungsten chloride and metallic aluminum were mixed evenly at a molar ratio of 1:1.6.
[0227] Under argon protection, the mixture was placed in a tube furnace and the heating temperature was set to 850 °C.
[0228] The temperature was heated at a rate of 20°C per minute to the target temperature and maintained for 4 hours for the reduction reaction.
[0229] 5. Post-processing
[0230] After the reduction reaction is completed, turn off the heating equipment and let the mixture cool naturally to room temperature. This process requires patience to ensure that the reaction is completed safely and avoid the danger of sudden cooling or the impact on product purity.
[0231] When the mixture is completely cooled, the reduced tungsten is taken out. At this point, the tungsten may still contain some unreacted impurities or residues and needs to be further cleaned.
[0232] The reduced tungsten is pickled with 10% hydrochloric acid for 1 hour. This step is to remove possible oxides or other impurities.
[0233] After pickling, the tungsten is rinsed several times with deionized water until the rinse solution is neutral to ensure that all residual acid and impurities are removed.
[0234] Put the rinsed tungsten into the drying oven, set the drying temperature to 80-100℃ and the drying time to 4 hours. The purpose of drying is to remove moisture and prevent the product from rusting or deterioration.
[0235] The dried tungsten is tested for purity. Purity testing can be performed by spectral analysis, chemical analysis or other appropriate methods. The purity should meet a predetermined standard, such as 99.999% or more.
[0236] It should be noted that, when preparing high-purity tungsten in this embodiment, the molybdenum content in tungsten is the focus of extraction and separation, and the specific extraction and separation includes:
[0237] After dissolving tungsten chloride in toluene, you can try to use a selective extractant to separate molybdenum chloride and tungsten chloride. This requires that the selected extractant has a higher affinity for molybdenum chloride and a lower affinity for tungsten chloride. However, in actual operation, the separation of tungsten chloride and molybdenum chloride may not be simple because their chemical properties are relatively similar.
[0238] One possible method is to optimize the separation effect by adjusting the type, concentration, pH value of the extractant and the extraction conditions (such as temperature, stirring speed, etc.).
[0239] Distillation or other separation techniques:
[0240] If the extraction separation effect is not ideal, you can consider using distillation, crystallization, ion exchange or other physical and chemical separation techniques to further purify the tungsten chloride, thereby indirectly reducing the molybdenum content.
[0241] Notes on post-processing:
[0242] During the reduction reaction and subsequent post-processing stages, it is necessary to ensure that the operating conditions do not reintroduce molybdenum impurities and to thoroughly wash and dry the product to prevent secondary contamination.
[0243] The method proposed in the fourth embodiment can also be used to purify tungsten. The purity of the purified tungsten should reach more than 99.999%.
[0244] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for purifying high-purity tantalum, characterized in that: The method comprises the following steps: Preparation of raw materials for purification of high purity tantalum; Carrying out chlorination reaction on the prepared raw materials; Separation and purification of raw materials after chlorination reaction; Reduction reaction; The raw material obtained after the reduction reaction is post-treated.
2. The method for purifying high-purity tantalum according to claim 1, characterized in that: The specific operations for preparing raw materials for high-purity tantalum purification include: Tantalum with a purity of at least 99.9% is selected as a raw material, and the mass of the raw material is 100 grams; Prepare to use a mechanical crusher to crush the raw material to a particle size between 60 and 80 meshes, and use tantalum powder as the raw material powder to obtain a uniformly distributed raw material powder.
3. The method for purifying high-purity tantalum according to claim 1, characterized in that: The specific operation of chlorination reaction of the prepared raw materials includes: Prepare a 1-liter reaction container and ensure that the inner wall of the container is clean and free of impurities; The crushed raw material powder is gently poured into the reaction kettle container, and the gas inlet and outlet and stirring device are installed; the waste chlorine recovery system after drying adopts the existing system: condensation in condenser - reuse in reflux recovery tank, tail gas alkaline water spray circulation absorption - activated carbon adsorption neutralization - up-to-standard discharge; Set the reaction temperature to 550°C and turn on the heating device at a heating rate of 10°C per minute; When the temperature reaches 550°C, the dried chlorine gas is introduced. The flow rate of the dried chlorine gas is set to 10 liters per hour and the continuous introduction time is 6 hours. While introducing the dried chlorine gas, turn on the stirring device and set the stirring speed to 100 revolutions per minute to ensure that the raw materials are fully in contact with the dried chlorine gas; After the chlorination reaction continued for 6 hours, the dried chlorine gas supply and the stirring device were turned off, and the dried chlorine gas in the reactor was replaced with argon gas, and then the reaction vessel was allowed to cool naturally to room temperature.
4. The method for purifying high-purity tantalum according to claim 1, characterized in that: The specific operations for separating and purifying the raw materials after the chlorination reaction include: The gas in the reaction vessel is discharged and the tantalum chloride therein is collected, the mass of the chloride being 80 g; Dissolve the chloride in 500 ml of carbon tetrachloride to obtain a uniform solution; The solution was extracted with dichloromethane as an extractant, the amount of the extractant was 300 ml, and the number of extractions was 3 times; The extracted solution was distilled at a temperature of 100° C. for 2 hours. The pure tantalum chloride obtained after distillation was collected, with a mass of 75 grams; The purity of chloride should be above 99.99%.
5. The method for purifying high-purity tantalum according to claim 1, characterized in that: The specific operations of the reduction reaction include: High-purity tantalum is obtained by aluminothermic reduction or vacuum carbon reduction.
6. The method for purifying high-purity tantalum according to claim 1, characterized in that: The specific operation of post-processing the raw material obtained after the reduction reaction includes: The reduced metal is pickled using 10% hydrochloric acid for 30 minutes; After pickling, use clean water to wash the metal several times with pure water and filter it until it is neutral; Put the washed metal into the drying oven, set the drying temperature to 80-100℃ and the drying time to 2 hours; The purity of the dried metal is tested and the purity should reach above 99.999%.