Palladium-based alloy ultrathin strip with high hardness and high conductivity, probe and preparation method of palladium-based alloy ultrathin strip

Through the specific composition and process processing of palladium-based alloy ultra-thin strip, combined with laser cutting, the contradiction between conductivity and mechanical properties of the probe material in high density and precision is solved, and the current resistance and resistance of the probe are improved. Fatigue and wear resistance improve the yield and detection reliability of the probe.

CN118910458AActive Publication Date: 2024-11-08贵研功能材料(云南)有限公司 +1

Patent Information

Application Number
CN202410954351.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

During the high density and precision process of existing probe materials, it is difficult to take into account high conductivity and excellent mechanical properties. Small surface defects and poor planarity affect the yield and detection reliability of the probe, and are resistant to high temperatures. Poor oxidation.

Method used

The palladium-based alloy ultra-thin strip is made of Pd, Cu, Ag, Ru and Pt in a specific proportion, and combined with melt casting, solid solution treatment, large deformation cold rolling, surface polishing and aging leveling processes, Pd-Ag solid solution is formed. Pd-Cu solid solution and CuPd ordered equal phases were prepared by laser cutting.

Benefits of technology

The probe with high hardness and high conductivity is achieved, with current resistance, fatigue resistance and wear resistance, which improves the yield of the probe and the reliability of wafer detection, and solves the surface quality and flatness problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910458A_ABST
    Figure CN118910458A_ABST
Patent Text Reader

Abstract

The invention discloses a high-hardness and high-conductivity palladium-based alloy ultrathin strip, a probe and a preparation method of the high-hardness and high-conductivity palladium-based alloy ultrathin strip. The palladium-based alloy ultrathin strip is composed of the following metal raw materials in percentage by mass: 46%-51% of Pd, 38.5%-42.5% of Cu, 8.5%-12.5% of Ag, 0.2%-3.0% of Ru and 0.1%-0.5% of Pt. The phase of the palladium-based alloy ultrathin strip is mainly composed of a Pd-Ag solid solution, a Pd-Cu solid solution, a CuPd ordered phase and a Cu3Pd ordered phase, and the average grain size of the palladium-based alloy ultrathin strip is 0.2-3 microns. Wherein Ru independently exists in a simple substance form and is in discontinuous fibrous distribution in a macroscopic area along the rolling direction. The finished product palladium-based alloy ultrathin strip can be directly used as a probe part, and the preparation method has the characteristics of high yield and high production efficiency; the vertical probe based on the palladium-based alloy ultrathin strip has the basic characteristics of high hardness, high strength, high conductivity, high elasticity, high surface quality and high planeness of the palladium-based alloy ultrathin strip, and shows the characteristics of excellent current resistance, fatigue resistance and wear resistance in a wafer test.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of alloy materials, and in particular relates to an ultra-thin strip of a palladium-based alloy with high hardness and high conductivity, a probe and a preparation method thereof. Background Art

[0002] The probe used in semiconductor wafer testing is the core component and consumable of wafer testing. It is used for precise connection between the wafer / pin to be tested and the tester, and has the functions of realizing signal transmission to detect current, conduction, etc. In order to meet the minimum spacing requirements, the probe size reaches the micron level, so the probe must have sufficient hardness, strength and elasticity, excellent current carrying capacity and stable contact resistance at high and low temperatures, so as to meet the requirements of probe structure design and use environment.

[0003] In addition to the urgent need to resolve the contradictory relationship between high conductivity and excellent mechanical properties, with the high density of integrated circuits and the precision of probes, tiny defects on the probe surface (such as scratches, pits, inclusions, etc.) and poor flatness (such as warping, edge waves, center waves, etc.) are likely to affect the probe yield and wafer detection reliability. For example, the probe may break during repeated contact with the wafer to be tested, the oxidation of the probe surface may affect the contact resistance, and the warping of the probe may affect the consistency of the probe arrangement and create an open circuit illusion. Therefore, higher requirements are placed on the surface quality and flatness of the materials used for the probes.

[0004] The physical and chemical properties of precious metal electrical contact materials are stable at high temperatures, overcoming the shortcomings of probe materials such as Be-Cu alloys with Au coatings that are easy to wear during use and Re-W alloys that have poor high-temperature oxidation resistance. Palladium-based alloys are the main alloy series of precious metal electrical contact materials. They have good high-temperature oxidation resistance and corrosion resistance. Through the combination of homogenization, solid solution strengthening, work hardening, and ordered phase transformation, they can simultaneously take into account high electrical conductivity and excellent mechanical properties. Through strip shape control and surface quality improvement, they can meet the requirements of probe materials for thickness uniformity, flatness, and surface quality. They are the probe materials with the best overall performance and the most potential.

[0005] The present invention aims to provide a high-hardness and high-conductivity palladium-based alloy ultra-thin strip, a probe and a preparation method thereof. Summary of the invention

[0006] The first object of the present invention is to provide a palladium-based alloy ultra-thin strip with high hardness and high conductivity. The second object of the present invention is to provide a method for preparing the palladium-based alloy ultra-thin strip. The third object of the present invention is to provide a probe based on the palladium-based alloy ultra-thin strip with current resistance, fatigue resistance and wear resistance.

[0007] The first object of the present invention is achieved by providing a high-hardness and high-conductivity palladium-based alloy ultra-thin strip, which is composed of the following metal raw materials in the following mass ratios: Pd 46%-51%, Cu 38.5%-42.5%, Ag 8.5%-12.5%, Ru 0.2%-3.0%, Pt 0.1%-0.5%; The phase of the palladium-based alloy ultra-thin strip is mainly composed of Pd-Ag solid solution, Pd-Cu solid solution, CuPd ordered phase, Cu3Pd Ordered phase composition, average grain size 0.2~3μm; In the palladium-based alloy ultra-thin strip, Ru exists independently in the form of a single substance and is distributed discontinuously in the form of fibers along the rolling direction in a macroscopic region. The diameter of the fibrous Ru is ≤400nm, and is mainly 100nm or less.

[0008] The second object of the present invention is achieved by the method for preparing the ultra-thin strip of palladium-based alloy with high hardness and high conductivity, which comprises the steps of melting and casting, solution treatment, large deformation cold rolling, surface polishing and cleaning, and aging and leveling treatment; The solution treatment and large deformation cold rolling process are carried out alternately, the alternating rolling times are not less than 3 times, and the total deformation of large deformation cold rolling is 80-97%; the solution treatment method is to keep the ingot obtained from the melting and casting process at 750-950°C for 2h in a vacuum furnace, and then cool it with N2 gas, with a cooling rate ≥15°C / s.

[0009] The third object of the present invention is achieved by providing a probe having current resistance, fatigue resistance and wear resistance based on the ultra-thin strip of palladium-based alloy with high hardness and high conductivity. The preparation method thereof is to laser cut the ultra-thin strip of palladium-based alloy to obtain the target probe.

[0010] The beneficial effects of the present invention are: 1. The finished palladium-based alloy ultra-thin strip provided by the present invention can be directly used as a probe part, and its preparation method has the characteristics of high yield and high production efficiency. The preparation method aims at the use characteristics of probe design, integration and wafer detection, abandons the conventional method such as improving the flatness in steps of profile aging treatment and leveling or straightening, but realizes aging and leveling simultaneously. In addition, the present invention attaches importance to the negative impact caused by poor surface quality of profiles and (or) probes, and incorporates the improvement of surface quality and flatness into the preparation process of ultra-thin strips. Therefore, the technical problems that may be encountered at the device end are circumvented from the material end, thereby improving the probe yield and the reliability of wafer detection.

[0011] 2. The vertical probe based on the palladium-based alloy ultra-thin strip provided by the present invention has the basic characteristics of high hardness, high strength, high conductivity, high elasticity, high surface quality and high flatness of the palladium-based alloy ultra-thin strip, and exhibits excellent current resistance, fatigue resistance and wear resistance in wafer testing. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 The present invention is a flow chart for preparing the palladium-based ultra-thin strip and probe; Figure 2 The figure is a comparison of the surface of the ultra-thin strip prepared in Example 1 of the present invention before and after polishing, wherein (a) and (c) are the overall effect picture and the microscopic effect picture of the unpolished strip surface, respectively; (b) and (d) are the overall effect picture and the microscopic effect picture of the polished strip surface, respectively; Figure 3 The schematic diagram of the aging treatment of the palladium-based ultra-thin strip of the present invention, wherein 1 is a vacuum heat treatment furnace; 2 is a palladium-based ultra-thin strip Strip; 3—leveling fixture; Figure 4 This is a microscopic morphology of fibrous Ru in the palladium-based ultra-thin strip prepared in Example 1 observed under a scanning electron microscope. DETAILED DESCRIPTION

[0013] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments, but the present invention is not limited in any way. Any changes or improvements made based on the teachings of the present invention fall within the protection scope of the present invention.

[0014] The invention discloses a high-hardness and high-conductivity palladium-based alloy ultra-thin strip, which is composed of the following metal raw materials in mass ratio: Pd 46%-51%, Cu 38.5%-42.5%, Ag 8.5%-12.5%, Ru 0.2%-3.0%, and Pt 0.1%-0.5%; The phase of the palladium-based alloy ultra-thin strip is mainly composed of Pd-Ag solid solution, Pd-Cu solid solution, CuPd ordered phase, Cu3Pd Ordered phase composition, average grain size 0.2~3μm; In the palladium-based alloy ultra-thin strip, Ru exists independently in the form of a single substance. After strong plastic deformation, the Ru dispersed in the matrix is ​​distributed in a discontinuous fibrous form along the rolling direction in a macroscopic area. The diameter of the fibrous Ru is 400nm or less, and is mainly 100nm or less.

[0015] The present invention selects palladium-silver-copper-ruthenium-platinum alloy as the alloy system of the probe material. In the five-element alloy, Ag and Cu can both play a role of solid solution strengthening in Pd, and an appropriate amount of Ag can reduce the high resistance effect caused by high Pd. Cu and Pd form CuPd and Cu3Pd ordered phases at low temperatures, which can significantly improve the conductivity and hardness. In this alloy system, Ru has a low solubility in Pd at low temperatures, so the Ru precipitation phase (solid solution) plays a role of dispersion strengthening; Pt not only has good oxidation resistance, but also can form Cu3Pt and CuPt ordered phases with Cu at low temperatures, playing a role of precipitation strengthening.

[0016] In order to improve the strength and hardness of the alloy as much as possible through solid solution strengthening and precipitation strengthening, and considering the anti-oxidation requirements of the probe material, the mass fraction ratio of Pd is 46%~51%, Cu is 38.5%~42.5%, and Ag is 8.5%~12.5%; while ensuring that the addition of Ru and Pt is harmless or (and) beneficial to the mechanical properties and electrical conductivity of the strip, while ensuring good processing and formability, Ru and Pt addition should be 0.2%~3.0% and 0.1%~0.5% respectively.

[0017] The palladium-based alloy ultra-thin strip has a Vickers hardness of 450-500 HV0.1, an electrical conductivity of 22-25% IACS, a tensile strength of 1100-1400 MPa, an elastic modulus of 110-160 GPa, a thickness of 30-60 μm, a thickness tolerance of ≤1 μm, no oxidation, no scratches, no pits on the surface, a metallic luster, and a surface roughness of R a ≤0.2μm, flatness ≤0.01mm.

[0018] The present invention also provides a method for preparing the high-hardness and high-conductivity palladium-based alloy ultra-thin strip, the preparation method comprising: Including melting casting, solution treatment, large deformation cold rolling, surface polishing and cleaning, aging and leveling treatment processes; 1. Melting and casting: It includes three steps: batching, smelting and casting. The selection of crucible, casting mold, melting power, holding time and remelting times during the melting and casting process is conducive to fully stirring the melt, reducing the segregation of alloy elements, removing gas impurities, and avoiding or reducing casting defects such as pores and shrinkage cavities. The inlet temperature of condensed water during casting is not higher than 20℃.

[0019] The smelting is carried out in a vacuum high-frequency induction furnace. Specifically, the raw materials are placed in a zirconia crucible and vacuum is drawn to maintain the vacuum degree at 10 -1Pa and below, fill with protective gas argon, increase the melting power to the melting temperature of 1200~1600℃, after all the raw materials are melted, keep warm for 8~12min, reduce the power to 0kw, after the surface of the melt solidifies, adjust the power again to make the temperature 1200~1600℃, and wait for the raw materials to melt again. The process from the solidification of the melt surface to the remelting is called remelting, and this process is repeated at least 2 times.

[0020] After smelting, it is cast into a copper mold and cooled and solidified into an alloy ingot, and the temperature of the condensate inlet is lower than 20°C.

[0021] 2. Solution treatment: refers to the alloy ingot being kept warm for a long time at high temperature in a vacuum heat treatment furnace, which can reduce the excessive stress inside the ingot, weaken the degree of Ag, Cu, Pt, and Ru segregation, play the role of solid solution strengthening and uniform organization, improve the processing of the ingot, and avoid cracking during the subsequent large deformation cold rolling process. The solution treatment holding temperature is 750~950℃, the holding time is 2h, and the annealing is carried out in a vacuum furnace and cooled by N2 gas, with a cooling rate of ≥15℃ / s.

[0022] 3. Large deformation cold rolling: Based on the analysis of the processing parameter window of the above palladium-based alloy, the rolling treatment is large deformation cold rolling, and the total rolling deformation is 80%~97%. Large deformation cold rolling has a strong effect of work hardening and grain refinement, making the submicron deposits arranged in fibrous form along the rolling direction.

[0023] Solution treatment and rolling are carried out alternately, the number of alternations is not less than 3 times, and the deformation of each pass is controlled at the same time, so as to avoid the problems of high probability of cracks caused by strong processing and low yield rate. Among them, the deformation of the first large deformation cold rolling pass is at most 20%, the deformation of the second large deformation cold rolling pass is at most 12%, and the deformation of the third and above large deformation cold rolling passes is at most 10%.

[0024] 4. Surface polishing and cleaning: This process is to solve the surface quality defects such as messy scratches, oxidation, stains, etc. introduced during the processing and heat treatment process. It includes two steps: surface polishing and ultrasonic cleaning.

[0025] 1) Surface polishing: A three-stage brush wheel continuous polishing device is used, with appropriate brush wheels and polishing media, to complete the rough polishing, medium polishing and precision polishing of ultra-thin strips in steps. Among them, the first-stage brush wheel is a nylon brush, the second and third-stage brush wheels are velvet brushes, the first and second-stage polishing media are 2.5~5μm diamond polishing liquid, the third-stage polishing medium is 0.05~1.5μm diamond polishing liquid, the brush wheel speed is 50~1000r / min, and the strip winding and unwinding speed is 2~15m / min.

[0026] 2) Ultrasonic cleaning: After polishing, the strip is further cleaned in an ultrasonic tank and dried.

[0027] 5. Aging and leveling treatment: The present invention is a strip tension aging treatment, specifically, the strip is fixed on the leveling fixture, placed in a vacuum heat treatment furnace for a certain period of time, and then cooled with N2, and the resulting finished strip is the finished strip. The heating rate is ≥1℃ / s, the insulation temperature is 350~420℃, the insulation time is 0.5~3h, and the cooling rate is ≤3℃ / min. The insulation temperature of 350~420℃ can induce and / or promote the ordered transformation, induce the precipitation of CuPd and / or Cu3Pd phases, thereby significantly improving the conductivity and hardness; on the other hand, the temperature range of 350℃~420℃ is very suitable for plate leveling. Above this temperature range, it is easy to cause serious loss of conductivity and (or) hardness, and below this temperature range, it is difficult to ensure the mechanical-electrical properties and leveling effect. The aging treatment simultaneously improves the hardness and conductivity of the strip and improves the flatness of the strip, solves the plate problems such as warping, edge waves, and middle waves, and kills two birds with one stone.

[0028] The present invention further provides a probe having current resistance, fatigue resistance and wear resistance based on the ultra-thin palladium-based alloy strip with high hardness and high conductivity. The preparation method thereof is to laser cut the ultra-thin palladium-based alloy strip to obtain the target probe.

[0029] Example 1 (1) Pd, Ag, Cu, Ru and Pt with a purity of 99.9% or above are mixed in a mass fraction of 47%, 12%, 39.5%, 1.2% and 0.3% respectively, and then melted and cast into alloy ingots in a vacuum high-frequency induction furnace. The specific steps are as follows: put the raw materials into a zirconia crucible, draw a vacuum, and the vacuum degree is 10 -1 Pa and below, fill with argon, increase the power to 1200℃, keep warm for 10 minutes after all the raw materials are melted, reduce the power to 0, wait for the surface of the melt to solidify, adjust the power to 1500℃ again, and remelt twice. After the smelting is completed, cast it into a copper mold to cool and solidify, and the temperature of the condensate inlet is not higher than 20℃.

[0030] (2) The obtained ingot was subjected to solution treatment followed by large deformation cold rolling three times alternately. The first solution treatment was carried out at 950℃ for 2h, in a vacuum furnace and cooled by N2 gas at a cooling rate of 15℃ / s, followed by the first large deformation cold rolling, with a total deformation of 91% and a pass deformation of 18%; the second solution treatment was carried out at 850℃ for 2h, in a vacuum furnace and cooled by N2 gas at a cooling rate of 15℃ / s, followed by the second large deformation cold rolling with a total deformation of 84% and a pass deformation of 10%; the third solution treatment was carried out at 800℃ for 2h, in a vacuum furnace and cooled by N2 gas at a cooling rate of 15℃ / s, followed by the third large deformation cold rolling with a total deformation of 86% and a pass deformation of 8%. The final processing was 0.04mm strip with a thickness tolerance of 1μm or less.

[0031] (3) The obtained strip is mechanically polished using three-stage brush wheels, wherein the first-stage brush wheel for surface polishing is a nylon brush, the second-stage and third-stage brush wheels are wool brushes, the first- and second-stage polishing media are 5μm diamond polishing liquid, the third-stage polishing medium is 1.5μm diamond polishing liquid, the brush wheel speed is 800r / min, and the strip winding and unwinding speed is 4m / min. After polishing, the strip is further cleaned and dried in an ultrasonic tank. Figure 2 It can be seen that the surface of the strip before polishing is grayish white and not bright enough after oxidation ( Figure 2 (a) ), with significant scratches ( Figure 2 (c) white line), the surface of the strip after polishing is bright metallic color ( Figure 2 (b)), and no scratches after polishing ( Figure 2 (d)).

[0032] (4) The cleaned strip is subjected to aging treatment to obtain the target ultra-thin strip. The specific method is to fix the strip on a self-made leveling fixture, put it into a vacuum heat treatment furnace, keep it at 400°C for 1 h, and heat up at a rate of 5°C / s. N2 cooling is used at a cooling rate of 1°C / min.

[0033] (5) The ultra-thin strip obtained in step (4) is cut into vertical probes by laser.

[0034] Example 2 (1) Pd, Ag, Cu, Ru and Pt with a purity of 99.9% or more are mixed in a vacuum high-frequency induction furnace at a mass fraction of 48.7%, 10%, 41%, 0.2% and 0.1% respectively, and then melted and cast into alloy ingots. The specific steps are as follows: put the raw materials into a zirconia crucible, draw a vacuum with a vacuum degree of 0.01MPa or less, fill with argon, increase the power to 1200℃, hold the temperature for 8 minutes after all the raw materials are melted, reduce the power to 0, and adjust the power to 1300℃ again after the surface of the melt solidifies, and remelt twice. After the smelting is completed, cast it into a copper mold to cool and solidify, and the temperature of the condensate inlet is not higher than 20℃.

[0035] (2) The obtained ingot was subjected to solution treatment followed by large deformation cold rolling three times alternately. The first solution treatment was carried out at 900℃ for 2h, in a vacuum furnace and cooled by N2 gas, with a cooling rate of 18℃ / s, followed by the first large deformation cold rolling, with a total deformation of 91% and a pass deformation of 20%; the second solution treatment was carried out at 850℃ for 2h, in a vacuum furnace and cooled by N2 gas, with a cooling rate of 18℃ / s, followed by the second large deformation cold rolling with a total deformation of 84% and a pass deformation of 12%; the third solution treatment was carried out at 850℃ for 2h, in a vacuum furnace and cooled by N2 gas, with a cooling rate of 18℃ / s, followed by the third large deformation cold rolling with a total deformation of 86% and a pass deformation of 10%. The final processing was 0.04mm strip with a thickness tolerance of 1μm or less.

[0036] (3) The obtained strips were mechanically polished using three-stage brush wheels, wherein the first-stage brush wheel for surface polishing was a nylon brush, the second-stage and third-stage brush wheels were wool brushes, the first- and second-stage polishing media were 5μm diamond polishing liquid, the third-stage polishing medium was 1.5μm diamond polishing liquid, the brush wheel speed was 800r / min, and the strip winding and unwinding speed was 4m / min. After polishing, the strip was further cleaned and dried in an ultrasonic tank.

[0037] (4) The cleaned strip is subjected to aging treatment to obtain the target ultra-thin strip. The specific method is to fix the strip on a self-made leveling fixture, put it into a vacuum heat treatment furnace, keep it at 350°C for 1 h, and the heating rate is 5°C / s. N2 cooling is used, and the cooling rate is 1°C / min.

[0038] (5) The ultra-thin strip obtained in step (4) is cut into vertical probes by laser.

[0039] Example 3 The method is basically the same as Example 1, except that in step (4), the cleaned ultra-thin strip is fixed on a homemade leveling fixture, placed in a vacuum heat treatment furnace, kept at 400°C for 3 h, with a heating rate of 5°C / s, and N2 cooling with a gas flow rate and a cooling rate of 3°C / min.

[0040] Comparative Example 1 Compared with Example 1, Comparative Example 1 is based on Pd 47% Ag 12% Cu 39.5% Ru 1.2% Pt 0.3% (mass fraction) processed into an ultra-thin strip. The difference between the preparation method of the ultra-thin strip and that of Example 1 is that the ingot obtained in step 1) is not subjected to the treatment of first solution treatment and then large deformation cold rolling alternately according to step 2), and the surface polishing and cleaning in step 3) and the leveling treatment in step 4) are not performed.

[0041] (1) Pd, Ag, Cu, Ru and Pt with a purity of 99.9% or more are prepared in mass fractions of 47%, 12%, 39.5%, 1.2% and 0.3% respectively, and then melted and cast into alloy ingots in a vacuum high-frequency induction furnace. The specific steps are as follows: put the raw materials into a zirconia crucible, draw a vacuum with a vacuum degree of 10-1Pa or less, fill with argon, increase the power to 1200°C, and after all the raw materials are melted, keep warm for 10 minutes, reduce the power to 0, and after the surface of the melt solidifies, adjust the power to 1500°C again, and remelt twice. After the smelting is completed, cast it into a copper mold to cool and solidify, and the temperature of the condensate inlet is not higher than 20°C.

[0042] (2) The obtained ingot is repeatedly solution treated and cold rolled to obtain a strip with a thickness of 0.04 mm and a thickness tolerance of 1 μm or less. The solution treatment is carried out in a vacuum furnace, and after being kept at 850°C for 2 hours, it is quickly water-cooled and then cold rolling is started.

[0043] (3) The obtained strip is subjected to aging treatment to obtain the target ultra-thin strip. The specific method is to fix the strip on a self-made leveling fixture, put it into a vacuum heat treatment furnace, keep it at 400°C for 1 h, with a heating rate of 5°C / s, and use N2 cooling at a cooling rate of 1°C / min.

[0044] (4) The ultra-thin strip obtained in step (3) is cut into vertical probes by laser.

[0045] Comparative Example 2 Compared with Example 1, Comparative Example 2 is based on Pd 40% Ag 30% Cu 30% The alloy is processed into an ultra-thin strip by the same method as in Example 1, and the strip is finally laser cut into vertical probes.

[0046] Test example The properties of the strips and probes prepared in Examples 1-3 and Comparative Examples 1-2 were tested, and the results are shown in Table 1.

[0047] Surface quality refers to the oxidation and scratches on the strip surface observed under a 20x microscope. The surface roughness is tested using a roughness meter, and the roughness is evaluated using the height characteristic parameter Ra as an indicator.

[0048] The flatness was tested with a feeler gauge, with a 000-grade marble platform as the sample table, and the maximum gap value between the sample to be tested and the sample table surface was used as the evaluation index.

[0049] Table 1 Performance of ultra-thin strips and probes in specific examples 1 to 3 and comparative examples 1 to 2 Note: “√” means the surface has metallic luster, no oxidation, no scratches, no pits or protrusions; “×” means the surface is dull, has surface defects such as oxidation, scratches, pits or bumps.

[0050] Results: From Table 1, it can be seen that the ultra-thin strips of Examples 1-3 have a Vickers hardness of 450-500 HV0.1, a conductivity of 22-25% IACS, a tensile strength of 1100-1400 MPa, an elastic modulus of 110-160 GPa, a thickness of 30-60 μm, a thickness tolerance of ≤1 μm, no oxidation, no scratches, no pits on the surface, a metallic luster, a surface roughness Ra ≤0.2 μm, and a flatness ≤0.01 mm. The probes obtained in Examples 1-3 all exhibit good current resistance, fatigue resistance, and wear resistance. Compared with Example 1, the preparation method of the ultra-thin strip in Comparative Example 1 is different, and the hardness and strength loss of the ultra-thin strip is large. At the same time, the ultra-thin strip is not surface polished, cleaned, or leveled. The probe prepared based on the strip is extremely unstable in the current carrying capacity, bending times, and wear resistance tests; while the ultra-thin strip obtained in Comparative Example 2 with different alloy components has significantly reduced hardness, strength, and conductivity, and the current carrying capacity, bending times, and wear resistance of the probe prepared based on the strip are also significantly reduced, and the current resistance is the current carrying capacity before the probe fails significantly as an evaluation index, and fatigue resistance refers to the ability of the probe to restore elasticity after bending, and the bending times are used as an evaluation index. Wear resistance is evaluated by the number of frictions corresponding to 50% wear of the probe tip. That is, the significant failure of the probe includes but is not limited to a significant decrease in the mechanical properties of the probe, severe deformation and oxidation of the probe, etc.

[0051] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.

Claims

1. A high-hardness and high-conductivity palladium-based alloy ultra-thin strip, characterized in that: It is composed of metal raw materials in the following mass ratios: Pd 46%~51%, Cu 38.5%~42.5%, Ag 8.5%~12.5%, Ru 0.2%~3.0%, Pt 0.1%~0.5%; The phase of the palladium-based alloy ultra-thin strip is mainly composed of Pd-Ag solid solution, Pd-Cu solid solution, CuPd ordered phase, and Cu3Pd ordered phase, and the average grain size is 0.2-3 μm; In the palladium-based alloy ultra-thin strip, Ru exists independently in the form of a single substance and is distributed discontinuously in the form of fibers along the rolling direction in a macroscopic region. The diameter of the fibrous Ru is ≤400nm, and is mainly 100nm or less.

2. The high-hardness and high-conductivity palladium-based alloy ultra-thin strip according to claim 1, characterized in that: The palladium-based alloy ultra-thin strip has a Vickers hardness of 450-500 HV0.1, an electrical conductivity of 22-25% IACS, a tensile strength of 1100-1400 MPa, an elastic modulus of 110-160 GPa, a thickness of 30-60 μm, a thickness tolerance of ≤1 μm, no oxidation, no scratches, no pits on the surface, a metallic luster, and a surface roughness of R a ≤0.2μm, flatness ≤0.01mm.

3. The method for preparing the ultra-thin strip of palladium-based alloy with high hardness and high conductivity according to claim 1, characterized in that: It includes melting and casting, solution treatment, large deformation cold rolling, surface polishing and cleaning, and aging and leveling treatment processes; The solution treatment and large deformation cold rolling process are carried out alternately, the alternating rolling times are not less than 3 times, and the total deformation of large deformation cold rolling is 80-97%; the solution treatment method is to keep the ingot obtained from the melting and casting process at 750-950°C for 2h in a vacuum furnace, and then cool it with N2 gas, with a cooling rate ≥15°C / s.

4. The method for preparing the ultra-thin strip of palladium-based alloy with high hardness and high conductivity according to claim 3, characterized in that: The aging and leveling treatment is a belt tension aging treatment, specifically, the strip is fixed on a leveling jig, placed in a vacuum heat treatment furnace, kept warm for a certain period of time, and then cooled using N2; the heating rate is ≥1°C / s, the holding temperature is 350~420°C, the holding time is 0.5~3h, and the cooling rate is ≤3°C / min.

5. The method for preparing the ultra-thin strip of palladium-based alloy with high hardness and high conductivity according to claim 3, characterized in that: The surface polishing and cleaning process is to polish through a three-stage brush wheel, and continuously complete the rough polishing, medium polishing, precision polishing and cleaning and drying of the strip with an ultrasonic pool; the first-stage brush wheel is a nylon brush, and the second and third-stage brush wheels are velvet brushes; the polishing medium used in the first and second stages is 2.5~5μm diamond polishing liquid, and the polishing medium used in the third stage is 0.05~1.5μm diamond polishing liquid, the brush wheel speed is 50~1000r / min, and the strip winding and unwinding speed is 2~15m / min.

6. The method for preparing the ultra-thin strip of palladium-based alloy with high hardness and high conductivity according to claim 3, characterized in that: The melting and casting process adopts a remelting process of no less than 2 times, and the melting process adopts argon protection, and the vacuum degree is ≤10 -1 Pa, melting temperature 1200~1600℃, melt holding time 8~12min.

7. The method for preparing the ultra-thin strip of palladium-based alloy with high hardness and high conductivity according to claim 3, characterized in that: The melting crucible used in the melting and casting process is a graphite crucible, the casting mold is a graphite mold, and the water inlet temperature of the condensed water during casting is not higher than 20°C.

8. A probe having current resistance, fatigue resistance and wear resistance based on the ultra-thin strip of palladium-based alloy with high hardness and high conductivity as described in claims 1-2, characterized in that: The preparation method of the probe is to perform laser cutting on the ultra-thin strip of palladium-based alloy to obtain the target probe.

Citation Information

Patent Citations

  • Electric brush with age-hardening effect and use thereof

    CN103757460A

  • Pd ALLOY FOR ELECTRIC / ELECTRONIC DEVICES

    CN104024448A

  • Palladium-based alloys

    CN108699629A

  • Alloy material for probe

    CN117015625A

  • Material for probe pin and probe pin

    JP2020002404A

Cited By

  • PdAgCuMt alloy and three-dimensional nano material prepared based on alloy

    CN120555859A