Aluminum alloy plate and preparation method thereof

By adding lithium, chromium, zirconium and other elements to the aluminum alloy sheet and adopting a specific process flow to form fine diffusion phases and refined grains, the problems of low strength of 6XXX series aluminum alloy and insufficient heat treatment of 5XXX series aluminum alloy are solved. It achieves high strength and lightweight effects and is suitable for structural parts such as automotive covers.

CN118910480APending Publication Date: 2024-11-08BINZHOU WEIQIAO NATIONAL SCIENCE & TECHNOLOGY ADVANCED TECHNOLOGY RESEARCH INSTITUTE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411129860.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

6XXX series aluminum alloy sheets have problems of low strength and insufficient lightweight in the automotive lightweight field. Moreover, 5XXX series aluminum alloy cannot be strengthened with heat treatment and strengthening, and the alloy has a low strength in the annealed state, making it difficult to meet the needs of high strength and lightweight. .

Method used

By adding lithium, chromium, zirconium and other elements to the aluminum alloy sheet, the process flow of vacuum smelting-casting-homogenization-hot rolling-cold rolling-solid solution-aging-ageing treatment is used to form δ′(Al3Li) and S′ (Al2MgLi) phase hinders dislocation movement and refines grains, improves the yield and tensile strength of the alloy, and reduces the alloy density.

Benefits of technology

It significantly improves the strength and lightweight weight reduction effect of aluminum alloy sheets, achieves higher yield strength and tensile strength, and has excellent forming performance and anisotropy, which is suitable for lightweight structural parts such as automotive covers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910480A_ABST
    Figure CN118910480A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of aluminum alloy materials, and discloses an aluminum alloy plate and a preparation method thereof. The aluminum alloy plate comprises the following components: silicon, iron, magnesium, lithium, manganese, chromium, zirconium, aluminum and other inevitable impurity elements. Wherein the lithium accounts for 0.8% to 1.5% in percentage by mass. By adding the lithium element into the aluminum alloy plate, the overall density of the alloy can be effectively reduced, so that the lighter aluminum alloy plate is prepared. Meanwhile, lithium and aluminum can form a delta '(Al3Li) phase and an S' (Al2MgLi) phase, and the precipitated phases have the characteristics of fine dispersion and can effectively hinder dislocation movement, so that the yield strength and the tensile strength of the alloy are improved. And moreover, the added elements such as chromium and zirconium refine crystal grains of the alloy, so that the plasticity of the material is improved, and the forming performance of the aluminum alloy can be further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of aluminum alloy materials, for example, to an aluminum alloy plate and a preparation method thereof. Background Art

[0002] In the field of automobile lightweighting, aluminum alloy body aluminum sheet is a very important application. Body sheet can be rolled from 2XXX, 5XXX, 6XXX and 7XXX series aluminum alloys. Except for 5XXX series aluminum alloys, the other three series aluminum alloys can be strengthened by heat treatment. Their strength can be further improved during painting and baking, and can be used to manufacture high-strength and high-rigidity outer panels.

[0003] Among them, although 2XXX series aluminum alloys and 7XXX series aluminum alloys have very high strength, they are not widely used due to their poor formability and corrosion resistance. 6XXX series aluminum alloys have good plastic forming properties and are used to manufacture complex-shaped structural parts. After forming, they can be artificially aged during the painting process. Therefore, 6XXX series aluminum alloys are currently the main research direction for body panels. However, 6XXX series aluminum alloy sheets still have the problems of low strength and insufficient lightness.

[0004] Compared with the above three aluminum alloy series, 5XXX series aluminum alloy has lower density and better formability. However, since 5XXX series aluminum alloy cannot be strengthened by heat treatment, the strength of the alloy is low in the annealed state and the weight is insufficient. Summary of the invention

[0005] In order to provide a basic understanding of some aspects of the disclosed embodiments, a brief summary is given below. The summary is not an extensive review, nor is it intended to identify key / critical components or delineate the scope of protection of these embodiments, but rather serves as a prelude to the detailed description that follows.

[0006] The embodiments of the present disclosure provide an aluminum alloy plate and a preparation method thereof, which improve the strength and lightweight effect of the aluminum alloy plate.

[0007] In some embodiments, an aluminum alloy plate is provided, the components of which include silicon, iron, magnesium, lithium, manganese, chromium, zirconium, aluminum and other inevitable impurity elements; wherein, in terms of mass percentage, lithium accounts for 0.8% to 1.5%.

[0008] Optionally, the aluminum alloy plate component also includes: indium, and the proportion of indium is 0.01% to 0.2% by mass.

[0009] Optionally, among the components of the aluminum alloy plate, by mass percentage, silicon accounts for 0.1% to 0.3%, iron accounts for 0.15% to 0.4%, magnesium accounts for 2.6% to 3.6%, manganese accounts for 0.05% to 0.3%, chromium accounts for 0.05% to 0.3%, zirconium accounts for 0.1% to 0.3%, and the balance is aluminum and other inevitable impurity elements.

[0010] In some embodiments, a method for preparing an aluminum alloy plate is provided, comprising: placing the raw materials of the aluminum alloy plate into a vacuum melting furnace, heating and melting the raw materials to obtain an aluminum melt; pouring the aluminum melt into a mold, and obtaining an ingot after solidification; homogenizing the ingot, and then hot rolling the ingot to obtain a hot-rolled plate; subjecting the hot-rolled plate to a first cold rolling, a solution treatment, a second cold rolling, and an aging treatment in sequence to obtain an aluminum alloy plate; wherein, in terms of mass percentage, the proportion of lithium in the aluminum alloy plate is 0.8% to 1.5%.

[0011] Optionally, the raw materials of the aluminum alloy plate include: aluminum ingots, magnesium ingots, lithium ingots, aluminum silicon alloys, iron agents, aluminum manganese alloys, aluminum chromium alloys, and aluminum zirconium alloys.

[0012] Optionally, in the aluminum alloy plate, by mass percentage, silicon accounts for 0.1% to 0.3%, iron accounts for 0.15% to 0.4%, magnesium accounts for 2.6% to 3.6%, manganese accounts for 0.05% to 0.3%, chromium accounts for 0.05% to 0.3%, zirconium accounts for 0.1% to 0.3%, and the balance is aluminum and other inevitable impurity elements.

[0013] Optionally, the raw material of the aluminum alloy plate further includes: aluminum-indium alloy, wherein, in terms of mass percentage, the proportion of indium in the aluminum alloy plate is 0.01% to 0.2%.

[0014] Optionally, the raw materials of the aluminum alloy sheet are placed in a vacuum melting furnace and heated and melted to obtain an aluminum melt, the steps comprising: placing the raw materials of the aluminum alloy sheet in a vacuum melting furnace and evacuating the furnace; after evacuating the furnace, filling with argon gas and heating and melting the furnace; during the heating process, stirring the melt to obtain an aluminum melt.

[0015] Optionally, before the step of pouring the aluminum melt into a mold and obtaining an ingot after solidification, the method further includes: adjusting the temperature of the aluminum melt to 690° C. to 720° C. and keeping the temperature for 2 to 5 minutes.

[0016] Optionally, the step of homogenizing the ingot includes: placing the ingot in an argon atmosphere protection furnace; heating the temperature in the furnace to 450° C. to 530° C., and keeping the temperature for 5 to 10 hours.

[0017] Optionally, before hot rolling, the preparation method further comprises: milling the ingot after homogenization treatment.

[0018] Optionally, hot rolling is performed to obtain a hot-rolled plate, the steps comprising: placing the ingot in an argon atmosphere protection furnace and heating it to 400°C to 450°C; after keeping warm for 1 to 2 hours, hot rolling is performed; wherein the hot rolling process has a pass reduction of 10% to 40%, and during the rolling process, the alloy temperature is maintained greater than or equal to 250°C.

[0019] Optionally, the step of performing a first cold rolling on the hot-rolled plate includes: performing a first cold rolling on the hot-rolled aluminum alloy plate; wherein the first cold rolling has a pass reduction of 20% to 50%.

[0020] Optionally, the step of performing solution treatment on the first cold-rolled plate includes: placing the first cold-rolled plate in a salt bath furnace and heating it to 480° C. to 550° C.; after keeping the temperature for 2 to 5 hours, quenching it in water.

[0021] Optionally, the step of performing a second cold rolling on the solution treated plate comprises: performing a single pass cold rolling on the solution treated plate with a deformation amount of 10% to 40%.

[0022] Optionally, the step of performing aging treatment on the plate after the second cold rolling includes: placing the plate after the second cold rolling in an aging furnace; heating the temperature in the furnace to 100° C. to 150° C., and keeping the temperature for 5 to 20 hours.

[0023] In some embodiments, an aluminum alloy sheet is provided, which is prepared using the method for preparing the aluminum alloy sheet described in any of the above technical solutions.

[0024] The aluminum alloy plate and the preparation method thereof provided by the embodiments of the present disclosure can achieve the following technical effects:

[0025] The components of the aluminum alloy sheet provided by the present disclosure include: silicon, iron, magnesium, lithium, manganese, chromium, zirconium, aluminum and other inevitable impurity elements; wherein, in terms of mass percentage, lithium accounts for 0.8% to 1.5%. By adding lithium to the aluminum alloy sheet, the overall density of the alloy can be effectively reduced, thereby preparing a lighter aluminum alloy sheet. At the same time, since lithium can form δ′ (Al3Li) phase and S′ (Al2MgLi) phase with aluminum, these precipitated phases have the characteristics of being fine and dispersed, which can effectively hinder the movement of dislocations, thereby improving the yield strength and tensile strength of the alloy. In addition, the addition of elements such as chromium and zirconium refines the grains of the alloy, improves the plasticity of the material, and thus can improve the forming properties of the aluminum alloy.

[0026] The aluminum alloy plate provided by the present disclosure has excellent strength performance and lightweight effect, and can be applied to vehicles.

[0027] The above general description and the following description are exemplary and explanatory only and are not intended to limit the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] One or more embodiments are exemplarily described by corresponding drawings, which do not limit the embodiments. Elements with the same reference numerals in the drawings are shown as similar elements, and the drawings do not constitute a scale limitation, and wherein:

[0029] Figure 1 It is a schematic diagram of a process for preparing an aluminum alloy plate provided by an embodiment of the present disclosure;

[0030] Figure 2 It is a schematic flow chart of another method for preparing an aluminum alloy plate provided by an embodiment of the present disclosure;

[0031] Figure 3 It is a schematic flow chart of another method for preparing an aluminum alloy plate provided by an embodiment of the present disclosure;

[0032] Figure 4 It is a schematic flow chart of another method for preparing an aluminum alloy plate provided by an embodiment of the present disclosure;

[0033] Figure 5 It is a schematic flow chart of another method for preparing an aluminum alloy plate provided by an embodiment of the present disclosure;

[0034] Figure 6 It is a schematic flow chart of another method for preparing an aluminum alloy plate provided in an embodiment of the present disclosure. DETAILED DESCRIPTION

[0035] In order to be able to understand the features and technical contents of the embodiments of the present disclosure in more detail, the implementation of the embodiments of the present disclosure is described in detail below in conjunction with the accompanying drawings. The attached drawings are for reference only and are not used to limit the embodiments of the present disclosure. In the following technical description, for the convenience of explanation, a full understanding of the disclosed embodiments is provided through multiple details. However, one or more embodiments can still be implemented without these details. In other cases, to simplify the drawings, well-known structures and devices can be simplified for display.

[0036] The terms "first", "second", etc. in the specification and claims of the embodiments of the present disclosure and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchanged where appropriate, so as to describe the embodiments of the embodiments of the present disclosure described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions.

[0037] In some embodiments, an aluminum alloy plate is provided, the components of which include silicon, iron, magnesium, lithium, manganese, chromium, zirconium, aluminum and other inevitable impurity elements, wherein, by mass percentage, lithium accounts for 0.8% to 1.5%.

[0038] The components of the aluminum alloy sheet provided by the present disclosure include: silicon, iron, magnesium, lithium, manganese, chromium, zirconium, aluminum and other inevitable impurity elements. Among them, the proportion of lithium is 0.8% to 1.5% in terms of mass percentage. By adding lithium to the aluminum alloy sheet, the overall density of the alloy can be effectively reduced, thereby preparing a lighter aluminum alloy sheet. At the same time, since lithium can form δ′(Al3Li) phase S′(Al2MgLi) phase with aluminum, these precipitated phases have the characteristics of fine dispersion, which can effectively hinder the movement of dislocations, thereby improving the yield strength and tensile strength of the alloy. In addition, the addition of elements such as chromium and zirconium refines the grains of the alloy, improves the plasticity of the material, and thus can improve the forming properties of the aluminum alloy.

[0039] The aluminum alloy plate provided by the present disclosure has excellent strength performance and lightweight effect, and can be applied to vehicles.

[0040] Optionally, the aluminum alloy sheet provided by the present disclosure can be used for lightweight structural parts such as body panels of vehicles.

[0041] Optionally, the specific proportion of lithium (Li) is 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4% or 1.5%.

[0042] Optionally, the aluminum alloy plate component also includes: indium, and indium (In) accounts for 0.01% to 0.2% by mass.

[0043] In this embodiment, by adding indium to the components of the aluminum alloy plate, a trace amount of In element is dissolved into the S′(Al2MgLi) phase, which can promote grain refinement. The fine grain structure helps to improve the strength and toughness of the material to improve the deformation ability of the alloy.

[0044] Optionally, the specific value of the proportion of indium is 0.01%, 0.03%, 0.05%, 0.07%, 0.09%, 0.1%, 0.15%, 0.18% or 0.2%.

[0045] Optionally, among the components of the aluminum alloy plate, by mass percentage, silicon accounts for 0.1% to 0.3%, iron accounts for 0.15% to 0.4%, magnesium accounts for 2.6% to 3.6%, manganese accounts for 0.05% to 0.3%, chromium accounts for 0.05% to 0.3%, zirconium accounts for 0.1% to 0.3%, and the balance is aluminum and other inevitable impurity elements.

[0046] In this embodiment, the strength, formability and lightweight effect of the aluminum alloy sheet are improved by reasonably selecting the mass proportion of each element. Specifically, the proportion of silicon (Si) is 0.1% to 0.3%, which enhances the strength and hardness of the aluminum alloy, especially during casting and aging. The proportion of iron (Fe) is 0.15% to 0.4% to improve the strength of the aluminum alloy, but the proportion of iron is not too high to ensure the corrosion resistance of the aluminum alloy sheet. The proportion of magnesium (Mg) is 2.6% to 3.6%, and an appropriate amount of magnesium can maintain good formability of the alloy. Moreover, magnesium is the main aging strengthening element, which can improve the strength and hardness of the aluminum alloy. The proportion of manganese (Mn) is 0.05% to 0.3%, and manganese can improve the strength and toughness of the aluminum alloy, while also improving the heat resistance of the alloy. The proportion of chromium (Cr) is 0.05% to 0.3%, and chromium is an important element to improve the corrosion resistance of aluminum alloys, and helps to refine the grains, thereby improving the mechanical properties of the material. Zirconium (Zr) accounts for 0.1% to 0.3%. Zirconium can increase the recrystallization temperature of aluminum alloys, which is beneficial to maintaining the work hardening effect. The balance is aluminum and other inevitable impurity elements. The content of each element in the inevitable impurity elements is less than or equal to 0.05%, and the total amount of other inevitable impurity elements is less than or equal to 0.15%.

[0047] In some embodiments, in combination Figure 1 A method for preparing an aluminum alloy plate is provided, comprising:

[0048] S101, placing the raw materials of the aluminum alloy plate into a vacuum melting furnace, heating and melting them to obtain an aluminum melt.

[0049] S102, pouring aluminum melt into a mold and obtaining an ingot after solidification.

[0050] S103, after homogenizing the ingot, hot rolling is performed to obtain a hot-rolled plate.

[0051] S104, the hot-rolled plate is subjected to a first cold rolling, a solution treatment, a second cold rolling, and an aging treatment in sequence to obtain an aluminum alloy plate.

[0052] Among them, calculated by mass percentage, the proportion of lithium in aluminum alloy plates is 0.8% to 1.5%.

[0053] The process steps of the preparation method for aluminum alloy sheet provided by the present disclosure include: vacuum melting-casting-homogenization treatment-hot rolling-first cold rolling-solution treatment-second cold rolling-aging treatment. By melting the raw materials through vacuum melting, impurities and gases can be effectively removed, thereby obtaining a high-purity aluminum melt. During the homogenization treatment of the ingot, Zr in the alloy will precipitate in the form of fine particles of β′ (Al3Zr), which will prevent dislocation slip and recrystallization during subsequent deformation and heat treatment, and improve the plasticity and uniformity of the ingot. The hot rolling process can effectively refine the grains and improve the strength and plasticity of the material. The fine grain structure also helps to improve the fatigue performance and corrosion resistance of the material. Through the first cold rolling, the grains can be further refined and a certain amount of work hardening can be introduced to improve the strength of the material. Solution treatment can dissolve alloy elements and provide conditions for subsequent aging strengthening. The second cold rolling further work-hardens the material and provides more nucleation sites for aging treatment. After aging treatment, a large amount of δ′(Al3Li) phase and S′(Al2MgLi) phase are precipitated in the alloy to achieve precipitation strengthening. The solution treatment and aging treatment in the preparation process can optimize the distribution and state of the alloy elements, ensuring that the alloy elements can fully exert their strengthening effect.

[0054] The aluminum alloy sheet prepared by the preparation method disclosed in the present invention has significantly improved strength and lower density compared to the existing 5XXX series aluminum alloy sheet and 6XXX series aluminum alloy sheet. Therefore, it has a very excellent lightweight effect. In addition, the aluminum alloy sheet prepared by the present invention also has good forming performance and anisotropy, and can be used for lightweight structural parts such as automobile covering parts.

[0055] Optionally, the raw materials of the aluminum alloy plate include: aluminum ingots, magnesium ingots, lithium ingots, aluminum silicon alloys, iron agents, aluminum manganese alloys, aluminum chromium alloys, and aluminum zirconium alloys.

[0056] Among them, calculated by mass percentage, in aluminum alloy plates, silicon accounts for 0.1% to 0.3%, iron accounts for 0.15% to 0.4%, magnesium accounts for 2.6% to 3.6%, manganese accounts for 0.05% to 0.3%, chromium accounts for 0.05% to 0.3%, zirconium accounts for 0.1% to 0.3%, and the remainder is aluminum and other inevitable impurity elements.

[0057] In this embodiment, the strength, formability and lightweight effect of the aluminum alloy sheet are improved by reasonably selecting the mass proportion of each element. Among them, by adding lithium to the aluminum alloy sheet, the overall density of the alloy can be effectively reduced, thereby preparing a lighter aluminum alloy sheet. At the same time, since lithium can form δ′ (Al3Li) phase and S′ (Al2MgLi) phase with aluminum, the above-mentioned precipitated phase has the characteristics of fine dispersion, which can effectively hinder the movement of dislocations, thereby improving the yield strength and tensile strength of the alloy. In addition, the addition of zirconium, chromium and other elements refines the grains of the alloy, improves the plasticity of the material, and thus can improve the forming performance of the aluminum alloy.

[0058] Specifically, silicon (Si) accounts for 0.1% to 0.3%, which enhances the strength and hardness of aluminum alloys, especially during casting and aging. Iron (Fe) accounts for 0.15% to 0.4% to improve the strength of aluminum alloys, but the proportion of iron is not too high to ensure the corrosion resistance of aluminum alloy sheets. Magnesium (Mg) accounts for 2.6% to 3.6%, and an appropriate amount of magnesium can maintain good formability of the alloy. Moreover, magnesium is the main aging strengthening element, which can improve the strength and hardness of aluminum alloys. Manganese (Mn) accounts for 0.05% to 0.3%, and manganese can improve the strength and toughness of aluminum alloys, while also improving the heat resistance of alloys. Chromium (Cr) accounts for 0.05% to 0.3%, and chromium is an important element to improve the corrosion resistance of aluminum alloys, and helps to refine grains, thereby improving the mechanical properties of materials. Zirconium (Zr) accounts for 0.1% to 0.3%, and zirconium can increase the recrystallization temperature of aluminum alloys, which is conducive to maintaining the work hardening effect. The balance is aluminum and other inevitable impurity elements. The content of each element in the inevitable impurity elements is less than or equal to 0.05%, and the total amount of other inevitable impurity elements is less than or equal to 0.15%.

[0059] Optionally, the raw material of the aluminum alloy plate further includes: aluminum-indium alloy, wherein, in terms of mass percentage, the proportion of indium in the aluminum alloy plate is 0.01% to 0.2%.

[0060] In this embodiment, by adding the element indium to the components of the aluminum alloy plate, grain refinement can be promoted, and the fine grain structure helps to increase the strength and toughness of the material, thereby improving the deformation ability of the alloy.

[0061] In some embodiments, in combination Figure 2 A method for preparing an aluminum alloy plate is provided, comprising:

[0062] S201, placing aluminum ingots, magnesium ingots, lithium ingots, aluminum silicon alloys, iron agents, aluminum manganese alloys, aluminum indium alloys, aluminum chromium alloys, and aluminum zirconium alloys into a vacuum melting furnace, and evacuating the furnace.

[0063] By smelting in a vacuum environment, gases and impurities in the aluminum melt can be removed during the smelting process, and the oxidation probability of easily oxidizable elements in the raw materials can be reduced.

[0064] S202, after completing the vacuuming, fill with argon gas and heat and melt.

[0065] Argon is flushed into the vacuum melting furnace. Argon is an inert gas that can form a protective atmosphere to prevent lithium from being oxidized.

[0066] S203, during the heating process, the melt is stirred to obtain an aluminum melt.

[0067] Continuous stirring during the heating process helps ensure that the alloying elements are evenly distributed in the melt and reduce component segregation. Stirring can also accelerate the melting process of the raw materials and make the melt reach a uniform melting state faster.

[0068] S204, pouring the aluminum melt into a mold and obtaining an ingot after solidification.

[0069] S205, after homogenizing the ingot, hot rolling is performed to obtain a hot-rolled plate.

[0070] S206, the hot-rolled plate is subjected to a first cold rolling, a solution treatment, a second cold rolling, and an aging treatment in sequence to obtain an aluminum alloy plate.

[0071] Among them, calculated by mass percentage, the proportion of lithium in aluminum alloy plates is 0.8% to 1.5%, and the proportion of indium is 0.01% to 0.2%.

[0072] In some embodiments, in combination Figure 3 A method for preparing an aluminum alloy plate is provided, comprising:

[0073] S301, placing aluminum ingots, magnesium ingots, lithium ingots, aluminum silicon alloys, iron agents, aluminum manganese alloys, aluminum indium alloys, aluminum chromium alloys, and aluminum zirconium alloys into a vacuum melting furnace, and evacuating the furnace.

[0074] S302, after completing the vacuuming, fill with argon gas and heat and melt.

[0075] S303, during the heating process, the melt is stirred to obtain aluminum melt.

[0076] S304, adjusting the temperature of the aluminum melt to 690° C. to 720° C. and keeping the temperature for 2 to 5 minutes, then pouring the aluminum melt into a mold and obtaining an ingot after solidification.

[0077] During the casting process, appropriate melt temperature and holding time help alloy elements fully dissolve in the aluminum melt, ensuring uniform composition of the ingot. In the temperature range of 690℃ to 720℃, the aluminum melt has good fluidity, which is conducive to the flow and filling of the melt in the mold and reduces casting defects. During the holding process, the gas in the melt has more time to escape, thereby reducing pores and other gas defects in the ingot.

[0078] Optionally, the temperature of the aluminum melt is adjusted to 690° C., 695° C., 700° C., 705° C., 710° C., 715° C. or 720° C. The specific value of the insulation time is 2 minutes, 3 minutes, 4 minutes or 5 minutes.

[0079] S305, placing the ingot in an argon atmosphere protection furnace, heating the temperature in the furnace to 450° C. to 530° C., and keeping the temperature for 5 to 10 hours to homogenize the ingot.

[0080] Homogenization treatment can eliminate the component segregation and as-cast structure inhomogeneity in the ingot, making the alloy elements more evenly distributed on a microscopic scale. By precisely controlling the heating temperature and holding time, the ingot can be made more uniform in microstructure. The temperature in the furnace is heated to 450°C to 530°C so that the alloy elements in the ingot can be better diffused, which helps to eliminate the component segregation inside the ingot and make the alloy elements more evenly distributed. It is conducive to the dissolution and uniform distribution of certain strengthening phases, thereby controlling the phase change. Keep warm for 5 to 10 hours to provide sufficient time for the diffusion of alloy elements to stabilize the microstructure of the ingot.

[0081] Optionally, the temperature in the furnace is heated to 450° C., 460° C., 470° C., 480° C., 490° C., 500° C., 510° C., 520° C. or 530° C. The specific value of the insulation time for the uniform post-treatment includes 5 hours, 6 hours, 7 hours, 8 hours, 9 hours or 10 hours.

[0082] S306, after homogenizing the ingot, hot rolling is performed to obtain a hot-rolled plate.

[0083] S307, the hot-rolled plate is subjected to a first cold rolling, a solution treatment, a second cold rolling, and an aging treatment in sequence to obtain an aluminum alloy plate.

[0084] Among them, calculated by mass percentage, the proportion of lithium in aluminum alloy plates is 0.8% to 1.5%, and the proportion of indium is 0.01% to 0.2%.

[0085] In some embodiments, in combination Figure 4 A method for preparing an aluminum alloy plate is provided, comprising:

[0086] S401, placing aluminum ingots, magnesium ingots, lithium ingots, aluminum silicon alloys, iron agents, aluminum manganese alloys, aluminum indium alloys, aluminum chromium alloys, and aluminum zirconium alloys into a vacuum melting furnace, and evacuating the furnace.

[0087] S402, after completing the vacuuming, fill with argon gas and heat and melt.

[0088] S403, during the heating process, the melt is stirred to obtain an aluminum melt.

[0089] S404, adjusting the temperature of the aluminum melt to 690° C. to 720° C. and keeping the temperature for 2 to 5 minutes, then pouring the aluminum melt into a mold and obtaining an ingot after solidification.

[0090] S405, placing the ingot in an argon atmosphere protection furnace, heating the temperature in the furnace to 450° C. to 530° C., and keeping the temperature for 5 to 10 hours to homogenize the ingot.

[0091] S406, after homogenizing the ingot, milling is performed.

[0092] S407, after milling, hot rolling is performed on the ingot to obtain a hot-rolled plate.

[0093] S408, the hot-rolled plate is subjected to a first cold rolling, a solution treatment, a second cold rolling, and an aging treatment in sequence to obtain an aluminum alloy plate.

[0094] Among them, calculated by mass percentage, the proportion of lithium in aluminum alloy plates is 0.8% to 1.5%, and the proportion of indium is 0.01% to 0.2%.

[0095] In the embodiments of the present disclosure, defects such as scale, cracks, inclusions, etc. may be formed on the surface of the ingot during the casting process. Milling can remove these surface defects and improve the surface quality of the ingot. The component segregation on the surface of the ingot is usually more serious than that inside. Milling can remove this part of the segregation area, thereby reducing the overall component segregation. By milling, the size and shape of the ingot can be accurately controlled to meet the requirements of subsequent processing for the dimensional accuracy of the ingot.

[0096] In some embodiments, in combination Figure 5 A method for preparing an aluminum alloy plate is provided, comprising:

[0097] S501, placing aluminum ingots, magnesium ingots, lithium ingots, aluminum silicon alloys, iron agents, aluminum manganese alloys, aluminum indium alloys, aluminum chromium alloys, and aluminum zirconium alloys into a vacuum melting furnace, and evacuating the furnace.

[0098] S502, after completing the vacuuming, fill with argon gas and heat and melt.

[0099] S503, during the heating process, the melt is stirred to obtain aluminum melt.

[0100] S504, pouring the aluminum melt into a mold and obtaining an ingot after solidification.

[0101] S505, placing the ingot in an argon atmosphere protection furnace and performing a homogenization treatment on the ingot.

[0102] S506, after homogenizing the ingot, milling is performed.

[0103] S507, after milling, hot rolling is performed on the ingot to obtain a hot-rolled plate.

[0104] S508, performing the first cold rolling on the hot-rolled plate.

[0105] S509, performing a solution treatment on the plate after the first cold rolling.

[0106] S510, performing a second cold rolling on the plate after the solution treatment.

[0107] S511, performing aging treatment on the plate after the second cold rolling to obtain an aluminum alloy plate.

[0108] Among them, calculated by mass percentage, the proportion of lithium in aluminum alloy plates is 0.8% to 1.5%, and the proportion of indium is 0.01% to 0.2%.

[0109] The process steps of the preparation method for aluminum alloy sheet provided by the present disclosure include: vacuum melting-casting-homogenization treatment-milling-hot rolling-first cold rolling-solution treatment-second cold rolling-aging treatment. The aluminum alloy sheet prepared by the preparation method of the present disclosure has significantly improved strength and lower density compared with the existing 5XXX series aluminum alloy sheet and 6XXX series aluminum alloy sheet. Therefore, it has a very excellent lightweight effect. In addition, the aluminum alloy sheet prepared by the present disclosure also has good formability and anisotropy, and can be used for lightweight structural parts such as automotive coverings.

[0110] Optionally, the step of hot rolling to obtain a hot-rolled plate comprises: placing the ingot in an argon atmosphere protection furnace and heating it to 400° C. to 450° C. After keeping the temperature for 1 to 2 hours, hot rolling is performed. The reduction amount of the hot rolling process is 10% to 40%, and during the rolling process, the alloy temperature is maintained at or above 250° C.

[0111] In this embodiment, the ingot is placed in an argon atmosphere protection furnace to prevent the ingot from oxidizing at high temperatures. Heated to 400°C to 450°C to improve the plasticity of the material for subsequent rolling. Insulated for 1 to 2 hours to ensure uniform temperature inside the ingot and reduce internal stress. Start hot rolling, and control the pass reduction at 10% to 40%. The appropriate pass reduction not only ensures the rolling efficiency, but also avoids excessive single deformation leading to material rupture. During the rolling process, the alloy temperature is kept greater than or equal to 250°C to ensure that the material has good plasticity, and the insulation process helps to evenly distribute the grains, reducing the uneven grains and internal stress inside the ingot. By heating and insulation, the plasticity of the material is improved, making the ingot easier to deform during the rolling process and reducing the risk of rupture.

[0112] Optionally, the specific value of the target heating temperature in the argon atmosphere protection furnace includes 400°C, 410°C, 420°C, 430°C, 440°C or 450°C. The specific value of the insulation time in the furnace includes 1 hour, 1.5 hours or 2 hours. During the rolling process, the alloy temperature is maintained greater than or equal to 250°C and less than 450°C, and the specific value can be 250°C, 300°C, 350°C, 400°C or 450°C.

[0113] Optionally, the specific value of the reduction amount per pass in the hot rolling process is 10%, 15%, 20%, 25%, 30%, 35% or 40%.

[0114] Optionally, the thickness of the hot-rolled plate has a value range of 3 mm to 5 mm. The specific value of the thickness of the hot-rolled plate can be determined by setting the hot-rolling process parameters according to the product structure requirements of the application scenario.

[0115] Optionally, the step of performing a first cold rolling on the hot-rolled sheet includes: performing a first cold rolling on the hot-rolled aluminum alloy sheet, wherein the first cold rolling has a pass reduction of 20% to 50%.

[0116] In this embodiment, according to the thickness of the plate after hot rolling and the target thickness after the first cold rolling, the first cold rolling pass reduction is determined to be 20% to 50%. By cold rolling the hot rolled plate, the plate is subjected to a large deformation during the cold rolling process to refine the grains, thereby improving the strength and hardness.

[0117] Optionally, the specific value of the reduction amount of the first cold rolling pass is 20%, 25%, 30%, 35%, 40%, 45% or 50%.

[0118] Optionally, the thickness of the plate after the first cold rolling ranges from 1.2 mm to 2 mm. The specific thickness of the plate after the first cold rolling can be set according to the product structure requirements of the application scenario by specifically setting the process parameters of the first cold rolling.

[0119] Optionally, the step of performing solution treatment on the first cold-rolled plate comprises: placing the first cold-rolled plate in a salt bath furnace and heating it to 480° C. to 550° C. After keeping the temperature for 2 to 5 hours, quenching it in water.

[0120] In this embodiment, a uniform heating environment is provided for the solution treatment by performing a solution treatment in a salt bath furnace. The temperature in the furnace is heated to 480°C to 550°C, which can effectively dissolve the strengthening elements in the alloy. And the temperature is kept at the target temperature for 2 to 5 hours, so that the strengthening elements are fully dissolved, the component segregation is reduced, and the alloy structure is more uniform. By performing a solution treatment on the cold-rolled plate, the strengthening elements in the alloy, such as magnesium and silicon, are fully dissolved in the aluminum matrix, providing conditions for subsequent aging treatment, thereby improving the strength and hardness of the material.

[0121] Optionally, the specific value of the target temperature in the salt bath furnace is 480° C., 490° C., 500° C., 510° C., 520° C., 530° C., 540° C. or 550° C. The specific value of the insulation time at the target temperature includes 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours or 5 hours.

[0122] Optionally, the step of performing a second cold rolling on the solution treated plate comprises: performing a single pass cold rolling on the solution treated plate with a deformation amount of 10% to 40%.

[0123] In this embodiment, after the solution treatment, the dislocation density in the alloy sheet is increased by cold deformation, the dispersion and uniformity of the aging precipitation phase are increased, the precipitation strengthening effect and plasticity of the alloy are improved, and the added trace In element also plays a role in promoting aging strengthening. Therefore, through the second cold rolling, the performance of the aluminum alloy sheet is further improved on the basis of the solution treatment. Specifically, the second cold rolling further refines the grains and improves the yield strength and tensile strength of the sheet. Cold rolling after the solution treatment helps to form a more uniform strengthening phase in the subsequent aging treatment, thereby improving the overall mechanical properties of the material. By accurately controlling the deformation amount of a single cold rolling, the target thickness can be achieved more accurately and the dimensional accuracy can be improved. In addition, the sheet after the second cold rolling has a more sensitive aging response, and better mechanical properties can be obtained after the aging treatment.

[0124] Optionally, the specific value of the reduction amount of the second cold rolling pass is 10%, 15%, 20%, 25%, 30%, 35% or 40%.

[0125] Optionally, the thickness of the plate after the second cold rolling ranges from 0.8 mm to 1.5 mm. The specific value of the thickness of the plate after the second cold rolling can be determined by setting the process parameters of the second cold rolling according to the product structure requirements of the application scenario.

[0126] Optionally, the step of performing aging treatment on the plate after the second cold rolling includes: placing the plate after the second cold rolling in an aging furnace, heating the temperature in the furnace to 100° C. to 150° C., and keeping the temperature for 5 to 20 hours.

[0127] In this embodiment, the temperature in the aging furnace is set between 100°C and 150°C, the plate after the second cold rolling is placed in the aging furnace, and heating is started. The temperature is kept at the set temperature for 5 to 20 hours. After aging treatment, a large amount of δ′ (Al3Li) and S′ (Al2MgLi) phases are precipitated in the alloy, among which the added trace In element promotes the effect of aging strengthening.

[0128] Optionally, specific values ​​of the furnace temperature in the aging furnace include: 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C or 150°C.

[0129] Specific values ​​of the insulation time for insulation in the furnace include: 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours or 20 hours.

[0130] In some embodiments, in combination Figure 6 As shown, a method for preparing an aluminum alloy plate is provided, comprising:

[0131] S601, placing aluminum ingots, magnesium ingots, lithium ingots, aluminum silicon alloy, iron agent, aluminum manganese alloy, aluminum indium alloy, aluminum chromium alloy, and aluminum zirconium alloy into a vacuum melting furnace, and evacuating the furnace.

[0132] S602, after completing the vacuuming, fill with argon gas and heat and melt.

[0133] S603, during the heating process, the melt is stirred to obtain aluminum melt.

[0134] S604, adjusting the temperature of the aluminum melt to 690° C. to 720° C. and keeping the temperature for 2 to 5 minutes, then pouring the aluminum melt into a mold and obtaining an ingot after solidification.

[0135] S605, placing the ingot in an argon atmosphere protection furnace, heating the temperature in the furnace to 450° C. to 530° C., and keeping the temperature for 5 to 10 hours to homogenize the ingot.

[0136] S606, after homogenizing the ingot, milling is performed.

[0137] S607, after milling, the ingot is placed in an argon atmosphere protection furnace and heated to 400°C to 450°C.

[0138] S608, after keeping the temperature for 1 to 2 hours, hot rolling is performed, wherein the reduction amount of each pass of the hot rolling process is 10% to 40%, and during the rolling process, the alloy temperature is maintained to be greater than or equal to 250°C.

[0139] S609, performing a first cold rolling on the hot-rolled aluminum alloy sheet, wherein the first cold rolling has a reduction of 20% to 50%.

[0140] S610, placing the plate after the first cold rolling in a salt bath furnace and heating it to 480°C to 550°C.

[0141] S611, after keeping at temperature for 2 to 5 hours, quench in water for solution treatment.

[0142] S612, single-pass cold rolling is performed on the plate after the solution treatment, and the deformation amount is 10% to 40%.

[0143] S613, placing the plate after the second cold rolling in an aging furnace.

[0144] S614, heating the temperature in the furnace to 100° C. to 150° C. and keeping the temperature for 5 to 20 hours to perform aging treatment to obtain an aluminum alloy plate.

[0145] Among them, calculated by mass percentage, the proportion of lithium in aluminum alloy plates is 0.8% to 1.5%, and the proportion of indium is 0.01% to 0.2%.

[0146] In some embodiments, an aluminum alloy sheet is provided, which is prepared using the method for preparing the aluminum alloy sheet described in any of the above technical solutions.

[0147] The aluminum alloy sheet provided by the present disclosure is prepared by the preparation method described in any of the above embodiments. Compared with the existing 5XXX series aluminum alloy sheet and 6XXX series aluminum alloy sheet, the strength is significantly improved and the density is lower. Therefore, it has a very excellent lightweight effect. In addition, the aluminum alloy sheet prepared by the present disclosure also has good forming performance and anisotropy, and can be used for lightweight structural parts such as automobile covering parts.

[0148] In combination with the method for preparing the aluminum alloy sheet provided in the above embodiment, several embodiments of preparing the aluminum alloy sheet are given below.

[0149] Embodiment 1:

[0150] Add aluminum ingots, magnesium ingots, lithium ingots, aluminum silicon alloys, iron agents, aluminum manganese alloys, aluminum chromium alloys, aluminum zirconium alloys, and aluminum indium alloys into the vacuum melting furnace, evacuate the furnace, fill it with argon gas for protection, heat and melt, and stir the melt evenly. Adjust the melt temperature to 700°C, keep it warm for 3 minutes, and then pour it into a metal mold equipped with a cooling water circulation system to cast a block ingot.

[0151] The ingot was homogenized at 520℃ in an argon atmosphere protection furnace for 8 hours, and the ingot was milled after homogenization. The ingot was heated to 440℃ in an argon atmosphere furnace for 2 hours, and then taken out for hot rolling, with a pass reduction of 10% to 40%, and the alloy temperature was kept ≥250℃ during the rolling process. The thickness of the rolled plate was 3mm.

[0152] The aluminum alloy sheet was cold rolled with a reduction of 20% to 50% per pass to obtain an aluminum alloy sheet with a thickness of 1.2 mm. The sheet was solution treated in a salt bath furnace at a heating temperature of 540° C. for 3 hours and then quenched in water.

[0153] The sheet was subjected to single-pass cold rolling to obtain an aluminum alloy sheet with a thickness of 0.8 mm. The aluminum alloy sheet was subjected to aging treatment in an aging furnace with a heating temperature of 120° C. and a holding time of 12 hours.

[0154] Embodiment 2:

[0155] Add aluminum ingots, magnesium ingots, lithium ingots, aluminum silicon alloys, iron agents, aluminum manganese alloys, aluminum chromium alloys, aluminum zirconium alloys, and aluminum indium alloys into the vacuum melting furnace, evacuate the furnace, fill it with argon gas for protection, heat and melt, and stir the melt evenly. Adjust the melt temperature to 700°C, keep it warm for 3 minutes, and then pour it into a metal mold equipped with a cooling water circulation system to cast a block ingot.

[0156] The ingot was homogenized at 520℃ in an argon atmosphere protection furnace for 8 hours. After homogenization, the ingot was milled. The ingot was heated to 440℃ in an argon atmosphere furnace for 2 hours, then taken out for hot rolling, with a pass reduction of 10% to 40%. During the rolling process, the alloy temperature was kept ≥250℃, and the thickness of the rolled plate was 4mm.

[0157] The aluminum alloy sheet was cold rolled with a reduction of 20% to 50% per pass to obtain an aluminum alloy sheet with a thickness of 1.5 mm. The sheet was solution treated in a salt bath furnace at a heating temperature of 540° C. for 4 hours and then quenched in water.

[0158] The sheet was subjected to single-pass cold rolling to obtain an aluminum alloy sheet with a thickness of 1.0 mm. The aluminum alloy sheet was subjected to aging treatment in an aging furnace with a heating temperature of 120° C. and a holding time of 12 hours.

[0159] Embodiment 3:

[0160] Add aluminum ingots, magnesium ingots, lithium ingots, aluminum silicon alloys, iron agents, aluminum manganese alloys, aluminum chromium alloys, aluminum zirconium alloys, and aluminum indium alloys into the vacuum melting furnace, evacuate the furnace, fill it with argon gas for protection, heat and melt, and stir the melt evenly. Adjust the melt temperature to 700°C, keep it warm for 3 minutes, and then pour it into a metal mold equipped with a cooling water circulation system to cast a block ingot.

[0161] The ingot was homogenized at 520℃ in an argon atmosphere protection furnace for 8 hours. After homogenization, the ingot was milled. The ingot was heated to 440℃ in an argon atmosphere furnace for 2 hours, then taken out for hot rolling, with a pass reduction of 10% to 40%. During the rolling process, the alloy temperature was kept ≥250℃, and the thickness of the rolled plate was 4mm.

[0162] The aluminum alloy sheet was cold rolled with a reduction of 20% to 50% per pass to obtain an aluminum alloy sheet with a thickness of 1.5 mm. The sheet was solution treated in a salt bath furnace at a heating temperature of 540° C. for 4 hours and then quenched in water.

[0163] The sheet was subjected to single-pass cold rolling to obtain an aluminum alloy sheet with a thickness of 1.2 mm. The aluminum alloy sheet was subjected to aging treatment in an aging furnace with a heating temperature of 120° C. and a holding time of 15 hours.

[0164] Several comparative examples for preparing aluminum alloy plates are given below.

[0165] Comparative Example 1:

[0166] Add aluminum ingots, magnesium ingots, aluminum silicon alloys, iron agents, aluminum manganese alloys, aluminum chromium alloys, and aluminum zirconium alloys into the vacuum melting furnace, evacuate the furnace, fill it with argon gas for protection, heat and melt, and stir the melt evenly. Adjust the melt temperature to 700°C, keep it warm for 3 minutes, and then pour it into a metal mold equipped with a cooling water circulation system to cast a block ingot.

[0167] The ingot was homogenized at 520℃ in an argon atmosphere protection furnace for 8 hours, and the ingot was milled after homogenization. The ingot was heated to 440℃ in an argon atmosphere furnace for 2 hours, and then taken out for hot rolling, with a pass reduction of 10% to 40%, and the alloy temperature was kept ≥250℃ during the rolling process. The thickness of the rolled plate was 4mm.

[0168] The aluminum alloy sheet was cold rolled with a reduction of 20% to 50% per pass to obtain an aluminum alloy sheet with a thickness of 1.0 mm. The sheet was annealed at a heating temperature of 340° C. for 1 hour and then air-cooled to room temperature.

[0169] Comparative Example 2:

[0170] Add aluminum ingots, magnesium ingots, lithium ingots, aluminum silicon alloys, iron agents, aluminum manganese alloys, aluminum chromium alloys, and aluminum zirconium alloys into the vacuum melting furnace, evacuate the furnace, fill it with argon gas for protection, heat and melt, and stir the melt evenly. Adjust the melt temperature to 700°C, keep it warm for 3 minutes, and then pour it into a metal mold equipped with a cooling water circulation system to cast a block ingot.

[0171] The ingot was homogenized at 520℃ in an argon atmosphere protection furnace for 8 hours, and the ingot was milled after homogenization. The ingot was heated to 440℃ in an argon atmosphere furnace, and then taken out for hot rolling after 2 hours of heat preservation. The pass reduction was 10% to 40%, and the alloy temperature was kept ≥250℃ during the rolling process. The thickness of the rolled plate was 4mm.

[0172] The aluminum alloy sheet was cold rolled with a reduction of 20% to 50% per pass to obtain an aluminum alloy sheet with a thickness of 1.5 mm. The sheet was solution treated in a salt bath furnace at a heating temperature of 540° C. for 4 hours and then quenched in water.

[0173] The sheet was subjected to single-pass cold rolling to obtain an aluminum alloy sheet with a thickness of 1.0 mm. The aluminum alloy sheet was subjected to aging treatment in an aging furnace with a heating temperature of 120° C. and a holding time of 12 hours.

[0174] The alloy compositions of the above embodiments and comparative examples are shown in Table 1.

[0175] Table 1 Alloy chemical composition (wt.%)

[0176] element Fe Si Mg Li Mn Cr Zr In Example 1 0.24 0.15 3.18 1.06 0.13 0.22 0.18 0.12 Example 2 0.27 0.16 3.12 1.1 0.15 0.16 0.21 0.15 Example 3 0.25 0.12 3.05 1.08 0.12 0.18 0.17 0.13 Comparative Example 1 0.22 0.15 3.22 - 0.23 0.25 0.15 - Comparative Example 2 0.27 0.16 3.15 1.12 0.15 0.15 0.18 -

[0177] The performance test results of the aluminum alloy plates of the above embodiments and comparative examples along the rolling direction are shown in Table 2.

[0178] Table 2 Aluminum alloy plate performance test results

[0179] Performance Indicators Tensile strength / MPa Yield strength / MPa Elongation / % <![CDATA[Density / (g / cm 3 )]]> Example 1 368 280 9.3 2.59 Example 2 362 267 9.8 2.58 Example 3 345 244 10.4 2.59 Comparative Example 1 221 107 23.5 2.68 Comparative Example 2 348 240 9.6 2.58

[0180] In Examples 1 to 3 shown in Table 1, the components of the aluminum alloy sheet, in addition to the inevitable impurities of aluminum, also include: iron, silicon, magnesium, lithium, manganese, chromium, zirconium, and indium. The alloy composition of Comparative Example 1 lacks lithium and indium relative to Examples 1 to 3. The alloy composition of Comparative Example 2 lacks indium relative to Examples 1 to 3.

[0181] The performance test results of the aluminum alloy plates obtained in the embodiments and comparative examples are shown in Table 2. Combining Table 2 with Table 1, it can be seen that the tensile strength and yield strength of Examples 1 to 3 are much higher than those of Comparative Example 1, and the elongation of Examples 1 to 3 is lower than that of Comparative Example 1. The comparison shows that the addition of lithium and indium to the alloy components, combined with the preparation method of the present application, improves the strength performance of the aluminum alloy plate and reduces the deformation. At the same time, the alloy density of Examples 1 to 3 is less than that of Comparative Example 1, which further illustrates that the aluminum alloy plate provided by the present disclosure is lighter and achieves the effect of lightweighting.

[0182] Combining Table 2 with Table 1, it can be seen that the yield strength of Examples 1 to 3 is higher than that of Comparative Example 2, and the difference in the other several properties is not large. Compared with Examples 1 to 3, Comparative Example 2 does not add indium, which means that the increase of indium can improve the yield strength of the aluminum alloy plate.

[0183] The above description and the accompanying drawings sufficiently illustrate the embodiments of the present disclosure to enable those skilled in the art to practice them. Other embodiments may include structural and other changes. The embodiments represent only possible variations. Unless explicitly required, individual components and functions are optional, and the order of operations may vary. Portions and features of some embodiments may be included in or replace portions and features of other embodiments. The embodiments of the present disclosure are not limited to the structures described above and shown in the accompanying drawings, and various modifications and changes may be made without departing from the scope thereof. The scope of the present disclosure is limited only by the appended claims.

Claims

1. An aluminum alloy plate, characterized in that: The components of aluminum alloy sheets include: silicon, iron, magnesium, lithium, manganese, chromium, zirconium, aluminum and other inevitable impurity elements; Among them, lithium accounts for 0.8% to 1.5% by mass.

2. The aluminum alloy sheet according to claim 1, characterized in that: The components also include: Indium, by mass percentage, accounts for 0.01% to 0.2%.

3. The aluminum alloy sheet according to claim 1 or 2, characterized in that: Among the components of aluminum alloy plates, by mass percentage, silicon accounts for 0.1% to 0.3%, iron accounts for 0.15% to 0.4%, magnesium accounts for 2.6% to 3.6%, manganese accounts for 0.05% to 0.3%, chromium accounts for 0.05% to 0.3%, zirconium accounts for 0.1% to 0.3%, and the balance is aluminum and other inevitable impurity elements.

4. A method for preparing an aluminum alloy sheet, characterized in that: include: The raw materials of the aluminum alloy sheet are placed in a vacuum melting furnace, heated and melted to obtain aluminum melt; The aluminum melt is poured into a mold and an ingot is obtained after solidification; After the ingot is homogenized, hot rolling is performed to obtain a hot-rolled plate; The hot-rolled plate is subjected to first cold rolling, solution treatment, second cold rolling and aging treatment in sequence to obtain an aluminum alloy plate; Among them, calculated by mass percentage, the proportion of lithium in aluminum alloy plates is 0.8% to 1.5%.

5. The preparation method according to claim 4, characterized in that: The raw materials of aluminum alloy plates include: aluminum ingots, magnesium ingots, lithium ingots, aluminum silicon alloy, iron agent, aluminum manganese alloy, aluminum chromium alloy, and aluminum zirconium alloy.

6. The preparation method according to claim 5, characterized in that: Calculated by mass percentage, in aluminum alloy plates, silicon accounts for 0.1% to 0.3%, iron accounts for 0.15% to 0.4%, magnesium accounts for 2.6% to 3.6%, manganese accounts for 0.05% to 0.3%, chromium accounts for 0.05% to 0.3%, zirconium accounts for 0.1% to 0.3%, and the balance is aluminum and other inevitable impurity elements.

7. The preparation method according to claim 4, characterized in that: The raw materials of the aluminum alloy sheet also include: aluminum-indium alloy, wherein, calculated by mass percentage, the proportion of indium in the aluminum alloy sheet is 0.01% to 0.2%.

8. The preparation method according to any one of claims 4 to 7, characterized in that The raw materials of the aluminum alloy sheet are placed in a vacuum melting furnace and heated and melted to obtain an aluminum melt. The steps include: The raw materials of the aluminum alloy sheet are placed in a vacuum melting furnace and vacuumized; After the vacuum is completed, argon gas is filled in and heated to melt; During the heating process, the melt is stirred to obtain an aluminum melt.

9. The preparation method according to any one of claims 4 to 7, characterized in that: Before the step of pouring the aluminum melt into a mold and obtaining an ingot after solidification, the process further includes: The temperature of the aluminum melt is adjusted to 690° C. to 720° C. and maintained at this temperature for 2 to 5 minutes.

10. The preparation method according to any one of claims 4 to 7, characterized in that: The steps of homogenizing the ingot include: The ingot is placed in an argon atmosphere protection furnace; Heat the temperature in the furnace to 450°C to 530°C and keep it at that temperature for 5 to 10 hours.

11. The preparation method according to any one of claims 4 to 7, characterized in that: Before hot rolling, it also includes: The ingot after homogenization treatment is milled.

12. The preparation method according to any one of claims 4 to 7, characterized in that: The steps of hot rolling to obtain hot rolled plates include: The ingot is placed in an argon atmosphere protection furnace and heated to 400°C to 450°C; After keeping the temperature for 1 to 2 hours, hot rolling is performed; The hot rolling process has a reduction of 10% to 40% per pass, and during the rolling process, the alloy temperature is maintained at greater than or equal to 250°C.

13. The preparation method according to any one of claims 4 to 7, characterized in that: The steps of first cold rolling of hot rolled plates include: The hot-rolled aluminum alloy sheet is subjected to the first cold rolling; The first cold rolling pass has a reduction of 20% to 50%.

14. The preparation method according to any one of claims 4 to 7, characterized in that: The steps of solution treatment of the first cold rolled plate include: The plate after the first cold rolling is placed in a salt bath furnace and heated to 480°C to 550°C; After keeping at temperature for 2 to 5 hours, quenching is performed in water.

15. The preparation method according to any one of claims 4 to 7, characterized in that: The steps of performing a second cold rolling on the solution treated plate include: The solution treated plate is cold rolled in a single pass with a deformation of 10% to 40%.

16. The preparation method according to any one of claims 4 to 7, characterized in that: The steps of aging treatment of the plate after the second cold rolling include: Placing the plate after the second cold rolling in an aging furnace; Heat the temperature in the furnace to 100°C to 150°C and keep it at that temperature for 5 to 20 hours.

17. An aluminum alloy plate, characterized in that: The aluminum alloy sheet is prepared by the preparation method of any one of claims 4 to 16.