Chloride ion corrosion resistant hot-rolled ribbed steel bar MG500C for anchor rod and production method of chloride ion corrosion resistant hot-rolled ribbed steel bar MG500C

By reasonably selecting trace elements and metallurgical processes in anchor steel bars, the hot-rolled ribbed steel bar MG500C with excellent chlorine ion corrosion resistance is solved, and the problems of cumbersome galvanizing processing and easy damage are achieved, achieving high corrosion resistance and low corrosion resistance Cost of anchor steel bar development.

CN118910505APending Publication Date: 2024-11-08山西建龙实业有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411040840.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The galvanized processing method used for anti-corrosion of anchor rod steel bars is cumbersome, and the transportation and construction process are prone to damage to the coating, resulting in difficult to improve corrosion resistance. In addition, domestic low-cost corrosion-resistant anchor rod steel bars are rarely studied.

Method used

A hot-rolled ribbed steel bar MG500C for an anchor with chlorine ion corrosion resistant to anchors, whose chemical composition includes trace elements such as C, Si, Mn, Cr, Ni, Cu, Mo, V, etc., through specific steel metallurgical processes, such as converter initial The process of refining, LF refining, billet continuous casting and rolling form the microstructure of bainite and ferrite, and improve the chloride ion corrosion resistance of the steel bars.

Benefits of technology

It has achieved significant improvement in the chloride corrosion resistance of anchor steel bars on the basis of ensuring mechanical properties, reduced the risk of plating damage, improved production efficiency and reliability, and is suitable for large-scale promotion and use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention belongs to the technical field of ferrous metallurgy, and particularly relates to a chloride ion corrosion resistant hot rolled ribbed bar MG500C for an anchor rod and a production method of the chloride ion corrosion resistant hot rolled ribbed bar MG500C. The corrosion-resistant steel bar is prepared from the following components in percentage by weight: less than or equal to 0.10 percent of C, 0.50 to 0.60 percent of Si, 1.30 to 1.40 percent of Mn, less than or equal to 0.020 percent of P, less than or equal to 0.010 percent of S, 2.50 to 2.60 percent of Cr, 0.55 to 0.65 percent of Ni, 0.48 to 0.52 percent of Cu, 0.13 to 0.15 percent of Mo, 0.09 to 0.10 percent of V and the balance of Fe and inevitable impurities. The production method comprises the steps of molten iron KR desulfurization, converter primary smelting, LF refining, square billet continuous casting, casting billet surface inspection and cleaning, heating and rolling. By controlling the contents of alloy elements such as C, Si, Mn, Cr, Ni, Cu, V and Mo and considering the strengthening and corrosion resisting mechanisms of all the elements, the corrosion resisting performance of the chloride ion corrosion resisting anchor rod steel bar is improved, the yield strength and the tensile strength are improved, and the cost is reduced. The microstructure is mainly bainite and ferrite; the Rp 0.2 is 525 to 550 MPa, the Rm is 730 to 790 MPa, and the A is 22.5 to 28 percent; and in a periodic infiltration corrosion test (a NaCl solution with the weight percentage of 2.0%), the relative corrosion rate is 70% or below.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of iron and steel metallurgy, and in particular relates to a chloride ion corrosion resistant hot-rolled ribbed steel bar MG500C for anchor rods and a production method thereof. Background Art

[0002] my country has a vast territory and rich mineral resources, which increases the demand for anchor steel. In recent years, with the development of society, people have put forward higher requirements for mining safety and the service life of supporting structures. Therefore, anchor steel bars are required to have not only good mechanical properties, but also good corrosion resistance. Under the premise of ensuring the mechanical properties of steel bars, corrosion-resistant anchor rods change the types of trace alloy elements contained therein, thereby changing the structure and chemical properties of the rust layer produced by the anchor rod in the chloride ion environment corrosion process, thereby inhibiting the corrosion process of the anchor rod steel bars and significantly improving the corrosion resistance of the anchor rod steel bars.

[0003] In recent years, China has also accelerated the research on anti-corrosion of anchor steel bars, and improved the corrosion resistance through galvanizing. However, the processing method is cumbersome, the production efficiency is low, and the coating is easily damaged during transportation and construction. The reliability is closely related to the construction level, and it is difficult to promote and use it on a large scale. There is little research on low-cost corrosion-resistant anchor steel bars in China, so it is very necessary to develop a low-cost, high-corrosion-resistant, and excellent mechanical property anchor steel bar. Summary of the invention

[0004] The purpose of the present invention is to provide a chloride ion corrosion resistant hot-rolled ribbed steel bar MG500C for anchor rods and a production method thereof, so as to solve the problem that the galvanizing process used for anti-corrosion of anchor rod steel bars is complicated and the coating is easily damaged during transportation and construction.

[0005] A chloride ion corrosion resistant hot-rolled ribbed steel bar MG500C for anchor rods, the chemical composition of which is measured by mass percentage: C: ≤0.10%, Si: 0.50-0.60%, Mn: 1.30-1.40%, P: ≤0.020%, S: ≤0.010%, Cr: 2.50-2.60%, Ni: 0.55-0.65%, Cu: 0.48-0.52%, Mo: 0.13-0.15%, V: 0.09-0.10%, the balance is Fe and unavoidable impurities, the microstructure is bainite and ferrite, the yield strength Rp 0.2 : 525-550MPa, tensile strength Rm: 730-790MPa, total elongation under maximum force A: 22.5-28%.

[0006] C is the most basic element of steel materials, playing the role of solid solution strengthening and carbide precipitation strengthening. However, the higher the C content, the worse the weldability and corrosion resistance of the steel; Si plays the role of solid solution strengthening to increase the strength of the steel and obtain a low yield ratio, but too high a content will significantly reduce the plasticity and toughness of the steel; Mn is a deoxidizer and desulfurizer, playing the role of solid solution strengthening to increase the strength of the steel and helping to improve the stability of austenite in the steel; too high a Mn content will cause segregation during casting, affecting the stability of the organizational structure, influencing the mechanical properties, and making the reinforcing bar have poor cold bending performance; V has the effects of precipitation strengthening and grain refinement, while increasing the strength and toughness of the steel, ensuring the elongation performance of the steel. At the same time, V also has the effect of refining grains, playing the role of pinning the austenite grain boundary and inhibiting the growth of austenite; Cr has been considered an effective element to improve the corrosion resistance to chloride ions, which can densify the rust layer, prevent the transmission of air and moisture into the steel matrix, increase the self-corrosion potential of the steel matrix and promote the passivation of the steel matrix.

[0007] The production method of the above-mentioned hot-rolled ribbed steel bar MG500C for anchor rods resistant to chloride ion corrosion includes the following steps: S1: KR desulfurization of hot metal: The conditions of blast furnace hot metal are controlled as follows, Si: 0.30 - 0.50%, P: ≤0.14%, S: ≤0.030%, temperature ≥1350°C; after the blast furnace hot metal arrives at the steelmaking workshop, CaO powder is sprayed into the hot metal ladle to promote the formation of CaS from S in the hot metal with CaO, and then the CaS slag is removed through slag skimming equipment; S2: Primary refining in converter: High-quality scrap steel is used to reduce the mixing of impurities. Copper-nickel alloy and molybdenum alloy are added into the furnace together with the scrap steel to ensure the uniformity of alloy components and reduce the alloy heat absorption temperature drop during tapping on the basis of saving production time. Slag materials are added during the converter blowing process, and the addition amount of each batch of slag materials ≤500 Kg. The slag materials must be added within 5 minutes of blowing to achieve early slag melting in the initial stage and complete slag melting during the process; the basicity of the final slag is controlled at R = 2.8 - 3.2, and the gun pressing time at the end point >30 s; bottom blowing nitrogen stirring is used in the early stage of the converter blowing process, and pure argon stirring is switched to in the middle and later stages. End point control: 0.04% < C < 0.05%. Strong bottom blowing stirring is carried out at the end of blowing, and the flow rate is controlled at 200 M 3The above ensures that the final molten steel is not oxidized when the carbon content is low; the tapping temperature of the converter is controlled at 1610℃~1630℃, and the final temperature is increased by 10-30℃ according to the ladle condition and abnormal conditions; use a ladle with good air permeability and clean turnover, open bottom nitrogen or argon 1-2 minutes before tapping, stir with a large amount of air during tapping to ensure that the alloy is fully melted, clean the turnover ladle to ensure red ladle tapping, and the ladle baking temperature is >900℃; slag blocking tapping to prevent large amounts of slag, and the slag layer thickness in the ladle is <50mm; deoxidation and alloying: first use a deoxidizer for deoxidation, and when one quarter of the steel is discharged, add a carburizer, silicon-manganese alloy and vanadium-nitrogen alloy in turn. When the molten steel is discharged to three quarters, add all the ingredients, and deoxidize and alloy in the ladle. Deoxidation is first ensured to ensure silicon-manganese alloy, VN The alloy recovery rate is stable, ensuring the good air permeability of the ladle bottom blowing air bricks; slag washing for tapping: when one quarter of the steel is discharged, lime, silica and slag washing materials are added with the steel flow during the tapping process, and the added amount is 5~6kg / t steel, which are added together with the alloy; argon is blown at the bottom of the steel tapping process throughout the whole process, and the stirring intensity is controlled during the stirring process. The exposed diameter of the molten steel on the ladle surface reaches 500mm, and at the same time, it is ensured that the temperature requirements before argon are met; after the ladle arrives at the argon station, it is blown for 3 minutes to take samples, and after adjusting the composition, argon is blown for 2 minutes to be hoisted for refining; S3: LF refining: When the ladle arrives at the refining site, the temperature is measured immediately and argon is passed. The argon pressure and flow rate are appropriate to slightly turn the slag surface without exposing the molten steel. 3 / 4 of FeCr alloy is added to solve the problem of insufficient melting and uneven composition of FeCr alloy caused by large amount of alloy in the steel-making process; sampling is taken after the first electrode is lowered, and the remaining 1 / 4 of FeCr alloy is added to adjust the composition; lime and fluorite are used to make slag, silicon carbide, calcium carbide, and aluminum chips are used for diffusion deoxidation and refining submerged arc, the refined slag is controlled, the slag is quickly turned into white slag, and soft argon blowing is performed; S4: Billet continuous casting: control the superheat to 15-30℃, use magnesium dry material in the middle ladle working layer, and the baking temperature is ≥1000℃; use a long nozzle from the large ladle to the middle ladle, and use a sealing cover for the middle ladle to reduce temperature drop and secondary oxidation; use an aluminum-carbon immersion nozzle from the middle ladle to the crystallizer to ensure verticality and centering, and the insertion depth of the immersion nozzle is 90±10 mm; use low-carbon acid-resistant steel protection slag for the crystallizer, and the protection slag must be dry and black-faced; use electromagnetic stirring in the production process, continuous casting cooling, the temperature before straightening is ≥900℃, ensure that the nozzle is not blocked, the water spray is uniform, and the position is centered to ensure the quality of the billet, and the surface is inspected and cleaned; S5: Heating: The temperature of the preheating section is ≤980℃. The heating temperature of the heating section and the soaking section is increased in the heating furnace. The furnace time is ≥120min to ensure that the alloy elements V, Mo, etc. are fully and evenly dissolved into the austenite matrix. S6: Rolling: In the rolling process, micro-pile or micro-drawing rolling is adopted for rough rolling and intermediate rolling, and loop tension-free rolling is adopted for finishing rolling to avoid drawing steel rolling. Air cooling process is adopted after rolling to improve the strength of steel without sacrificing toughness, promote grain refinement, increase the yield strength and tensile strength of the material, improve the uniformity of the organization, and help to obtain a more uniform microstructure.

[0008] Preferably, the slag material in step S2 includes lime, dolomite and temperature regulating material, with lime accounting for 2 / 3 of the first batch, 1 / 3 of the later batch, all of the dolomite, 3 / 4 of the temperature regulating material being added, and the rest being adjusted during "re-drying".

[0009] Preferably, the soft argon blowing time in step S3 shall not be less than 15 minutes.

[0010] Preferably, the continuous casting cooling in step S4 adopts a slow cooling mode, which reduces the amount of cooling water by 10% compared with conventional cooling water.

[0011] Preferably, in step S5, the temperature of the heating section is controlled at 1140±20°C, and the temperature of the soaking section is controlled at 1160±20°C.

[0012] Preferably, in step S6, the starting rolling temperature of the rough rolling is 1060±20°C, and the finishing rolling temperature is 940±20°C.

[0013] Preferably, in step S6, pre-watering treatment is performed during the rolling process, no watering is performed after rolling, and the cooling rate of air cooling after rolling is controlled at 1-2°C / s.

[0014] Compared with the prior art, the present invention has the following beneficial effects: The production method of the present invention controls the content of C, Si, Mn, V, Ni, Cu and Mo alloy elements in the converter primary refining to ensure the uniformity of alloy components and reduce the alloy endothermic temperature drop in the steel-making process; FeCr is added in the refining furnace to solve the problems of insufficient melting and uneven composition of FeCr alloy caused by a large amount of alloy in the steel-making process; by controlling the content of C, Si, Mn, Cr, Ni, Cu, V and Mo alloy elements, the Cr, Ni and Mo element component system is optimized to increase the strength of the steel bar; lime + fluorite is used for slag making, and the refining process is kept Prove the refining submerged arc operation; adopt the process of "process water penetration + air cooling after rolling", reasonably control the heating temperature, the start rolling temperature of rough rolling, the finishing rolling temperature and the cooling method, the obtained steel bars have good strength and toughness, excellent chloride ion corrosion resistance, start rolling at high temperature, reduce the wear of the rolls, extend the service life of the rolls, help to obtain finer grains, improve the microstructure of the material, make the steel bar structure low-carbon bainite, improve the mechanical properties, and at high temperature the plasticity of the steel billet increases, the deformation resistance decreases, making the rolling process easier and reducing energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The microstructure diagram of the φ22mm chloride ion corrosion resistant anchor steel bar in the embodiment; Figure 2 This is a corrosion external morphology of the corrosion sample after the φ22mm chloride ion corrosion resistant anchor steel bar in the embodiment was immersed in a NaCl solution with a concentration of 0.340 mol / L for 72 hours; Figure 3 This is the external morphology of the corrosion of the ordinary steel bar after being immersed in a NaCl solution with a concentration of 0.340 mol / L for 72 hours. DETAILED DESCRIPTION

[0016] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0017] A method for producing hot-rolled ribbed steel bars resistant to chloride ion corrosion for anchor rods comprises the following steps: S1: Hot metal KR desulfurization: The conditions of hot metal in blast furnace are controlled as follows: Si: 0.30%, P: 0.14%, S: 0.030%, and the temperature is 1350℃; after the hot metal in blast furnace arrives at the steelmaking workshop, CaO powder is sprayed into the hot metal ladle to promote the S in hot metal to react with CaO to generate CaS, and then the CaS slag is removed by slag removal equipment; S2: Converter primary refining: Use high-quality scrap steel to reduce impurities. Copper-nickel alloy and molybdenum alloy are added into the furnace together with scrap steel. Lime, dolomite and temperature regulating materials are added during converter blowing. Lime is 2 / 3 of the first batch, 1 / 3 of the later batch, all of dolomite, and 3 / 4 of temperature regulating materials are added. The amount of slag added to each batch is 480Kg. The slag must be added within 5 minutes of blowing to achieve early slag formation in the early stage and thorough slag formation during the process. The final slag basicity is controlled at R=2.8, and the terminal gun pressure time is 40 s. Bottom blowing nitrogen stirring is used in the early stage of converter blowing, and pure argon stirring is switched in the middle and late stages. The terminal control: C is 0.045%, and bottom blowing strong stirring is carried out at the end of blowing, and the flow rate is controlled at 220M 3, to ensure that the final molten steel is low in carbon and not oxidized; the converter tapping temperature is controlled at 1610℃~1630℃, and the final temperature is increased by 10℃ according to the ladle condition and abnormal conditions; a ladle with good air permeability and clean turnover is used, and bottom nitrogen is blown 2 minutes in advance before tapping. A large amount of stirring is used during the tapping process to ensure that the alloy is fully melted, and the red envelope is tapped. The ladle baking temperature is 910℃; slag blocking tapping, prevent a large amount of slag, and the slag layer thickness in the ladle is <50mm; deoxidation and alloying: first use a deoxidizer for deoxidation, and when a quarter of the steel is discharged, add a carburizer, silicon-manganese alloy and vanadium-nitrogen alloy in turn. When the molten steel is discharged to three-quarters, add all the additions, and deoxidation and alloying are carried out in the ladle. Deoxidation is first ensured to ensure silicon-manganese alloy and VN alloy The yield is stable, ensuring the good air permeability of the ladle bottom blowing air bricks; slag washing for tapping: when one quarter of the steel is discharged, lime, silica and slag washing materials are added with the steel flow during the tapping process, and the added amount is 5kg / t steel, which is added together with the alloy; argon is blown at the bottom of the steel tapping process throughout the whole process, and the stirring intensity is controlled during the stirring process. The exposed diameter of the molten steel on the ladle surface reaches 500mm, and at the same time, it is ensured that the temperature requirements before argon are met; after the ladle arrives at the argon station, it is blown for 3 minutes to take samples, and after adjusting the composition, argon is blown for 2 minutes to be hoisted for refining; S3: LF refining: When the ladle arrives at the refining site, the temperature is measured immediately and argon is passed. The argon pressure and flow rate are suitable for slightly turning the slag surface without exposing the molten steel. 3 / 4 of FeCr alloy is added to solve the problem of insufficient melting and uneven composition of FeCr alloy caused by large amount of alloy in the steel-making process; sampling is taken after the first electrode is lowered, and the remaining 1 / 4 of FeCr alloy is added to adjust the composition; lime and fluorite are used to make slag, silicon carbide, calcium carbide and aluminum chips are used for diffusion deoxidation and refining submerged arc, the refined slag is controlled, the slag is quickly turned into white slag, and soft argon blowing is carried out for 15 minutes; S4: Billet continuous casting: control the superheat at 15℃, use magnesium dry material in the middle ladle working layer, and the baking temperature is 1080℃; use a long nozzle from the large ladle to the middle ladle, and use a sealing cover for the middle ladle to reduce temperature drop and secondary oxidation; use an aluminum-carbon immersion nozzle from the middle ladle to the crystallizer to ensure verticality and centering, and the insertion depth of the immersion nozzle is 90 mm; use low-carbon acid-resistant steel protection slag for the crystallizer, and the protection slag must be dry and black-faced; use electromagnetic stirring in the production process; use slow cooling mode for continuous casting cooling, and the temperature before straightening is 960℃ to ensure that the nozzle is not blocked, the water spray is uniform, and the position is centered to ensure the quality of the billet, and the surface is inspected and cleaned; S5: Heating: The preheating section temperature is 970°C. The heating section and soaking section temperatures are increased in the heating furnace. The heating section temperature is controlled at 1160°C, the soaking section temperature is controlled at 1140°C, and the furnace time is 120 minutes to ensure that the alloy elements V, Mo, etc. are fully and evenly dissolved in the austenite matrix. S6: Rolling: Micro-pile or micro-drawing rolling is adopted for rough and medium rolling in the rolling process. The starting rolling temperature of rough rolling is 1090℃. Loopless tension-free rolling is adopted for finishing rolling to avoid drawing steel. The finishing temperature is 930℃. Air cooling process is adopted after rolling. The cooling rate is controlled at 1℃ / s. Pre-water penetration treatment is carried out during rolling, and no water penetration is carried out after rolling. The strength of steel is improved without sacrificing toughness, grain refinement is promoted, the yield strength and tensile strength of the material are improved, the uniformity of the organization is improved, and it is helpful to obtain a more uniform microstructure.

[0018] The chloride ion corrosion-resistant hot-rolled ribbed steel bars for anchor rods prepared by the above production method have chemical compositions, by mass percentage, including: C: 0.09%, Si: 0.55%, Mn: 1.35%, P: 0.018%, S: 0.009%, Cr: 2.51%, Ni: 0.57%, Cu: 0.49%, Mo: 0.14%, V: 0.09%, and the balance is Fe and unavoidable impurities.

[0019] Anchor rods usually use φ22mm steel bars. The yield strength of the φ22mm steel bars prepared by the above method is 550MPa, the tensile strength is 750MPa, and the total elongation under maximum force is 23.5%. Figure 1 As shown in Figure 2, the microstructure of the steel bar is low-carbon bainite and ferrite. Figure 2 As shown in the figure, the average corrosion rate of the accelerated corrosion test was 3.3245 g / (m 2 h), the relative corrosion rate is 54.5%; Figure 3 As shown in the figure, the corrosion external morphology of the corrosion sample after the ordinary steel bar was immersed in a NaCl solution with a concentration of 0.340 mol / L for 72 hours.

[0020] The steel bars prepared by the production method have a yield strength of 525-550MPa, a tensile strength of 730-790MPa, a total elongation of 22.5-28% under maximum force, and an average corrosion rate of 2.2635-3.843g / (m2·h) in an accelerated corrosion test in a NaCl solution with a concentration of 0.340mol / L for 72 hours, and a relative corrosion rate of less than 70%. According to the results of the accelerated corrosion test, the chloride ion corrosion resistance is enhanced, and the yield strength and tensile strength are increased.

Claims

1. A hot-rolled ribbed steel bar MG500C for anchor rods resistant to chloride ion corrosion, characterized in that: The chemical composition is calculated by mass percentage, including: C: ≤0.10%, Si: 0.50-0.60%, Mn: 1.30-1.40%, P: ≤0.020%, S: ≤0.010%, Cr: 2.50-2.60%, Ni: 0.55-0.65%, Cu: 0.48-0.52%, Mo: 0.13-0.15%, V: 0.09-0.10%, the balance is Fe and unavoidable impurities, the microstructure is bainite and ferrite, the yield strength is Rp 0.2 : 525-545MPa, tensile strength Rm: 730-790MPa, total elongation under maximum force A: 22.5-28%.

2. The production method of the chloride ion corrosion resistant hot-rolled ribbed steel bar MG500C for anchor rods according to claim 1, characterized in that: The following steps are involved: S1: Hot metal KR desulfurization: The conditions of hot metal in blast furnace are controlled as follows: Si: 0.30-0.50%, P: ≤0.14%, S: ≤0.030%, temperature ≥1350℃; after the hot metal in blast furnace arrives at the steelmaking workshop, CaO powder is sprayed into the hot metal ladle to promote the S in the hot metal to react with CaO to generate CaS, and then the CaS slag is removed by slag removal equipment; S2: Primary steelmaking in the converter: High-quality scrap steel is used to reduce the mixing of impurities. The copper-nickel alloy and molybdenum alloy are added into the furnace together with the scrap steel. On the basis of saving production time, the uniformity of alloy components is ensured, and the temperature drop caused by alloy heat absorption during tapping is reduced. Slag materials are added during the converter blowing process. The addition amount of slag materials per batch ≤ 500 Kg, and the slag materials must be added within 5 minutes of blowing to achieve early slag melting in the initial stage and complete slag melting in the process; the basicity of the final slag is controlled at R = 2.8 - 3.2, and the gun lowering time at the end point > 30 s; bottom blowing nitrogen stirring is adopted in the early stage of the converter blowing process, and pure argon stirring is switched in the middle and later stages. End point control: 0.04% < C < 0.05%. Bottom blowing strong stirring is carried out at the end of blowing, and the flow rate is controlled at 200 M 3 Above, ensure that the molten steel at the end point is not over-oxidized under the condition of low carbon; the tapping temperature of the converter is controlled at 1610℃ - 1630℃, and the end point temperature is increased by 10 - 30℃ according to the ladle condition and abnormal situation; use a ladle with good air permeability of the porous plug and clean turnover. Open the bottom blowing nitrogen or argon 1 - 2 minutes before tapping. Stir vigorously during tapping to ensure full melting of the alloy. The clean turnover ladle ensures tapping with a hot ladle, and the ladle baking temperature > 900℃; slag blocking during tapping to prevent a large amount of slag from flowing down, and the thickness of the slag layer in the ladle < 50 mm; deoxidation and alloying: First, use a deoxidizer for deoxidation. When one-fourth of the steel is discharged, add a carburizer, ferrosilicon manganese alloy, and vanadium nitride alloy in sequence, and finish adding when three-fourths of the steel is discharged. Deoxidation and alloying are carried out in the ladle. First, deoxidize to ensure the stable recovery rate of ferrosilicon manganese alloy and VN alloy, and ensure good air permeability of the bottom blowing porous plug of the ladle; slag washing during tapping: When one-fourth of the steel is discharged, add lime, silica, and slag washing materials along with the steel flow during tapping. The addition amount is 5 - 6 kg / t of steel, and add them together with the alloy; Stir with bottom blowing argon throughout the tapping process, control the stirring intensity during the stirring process, and the exposed diameter of the molten steel on the ladle surface reaches 500 mm, while ensuring that the pre-argon temperature requirement is met; After the ladle arrives at the argon station, blow for 3 minutes for sampling, adjust the composition, and then blow argon for 2 minutes and lift the ladle to the refining station; S3: LF refining: When the ladle arrives at the refining site, the temperature is measured immediately and argon is passed. The argon pressure and flow rate are suitable for slightly turning the slag surface without exposing the molten steel. 3 / 4 of FeCr alloy is added to solve the problem of insufficient melting and uneven composition of FeCr alloy caused by large amount of alloy in the steel-making process; sampling is taken after the first electrode is lowered, and the remaining 1 / 4 of FeCr alloy is added to adjust the composition; lime and fluorite are used to make slag, silicon carbide, calcium carbide, and aluminum chips are used for diffusion deoxidation and refining submerged arc, the refined slag is controlled, the slag is quickly turned into white slag, and soft argon blowing is performed; S4: Billet continuous casting: control the superheat to 15-30℃, use magnesium dry material in the middle ladle working layer, and the baking temperature is ≥1000℃; use a long nozzle from the large ladle to the middle ladle, and use a sealing cover for the middle ladle to reduce temperature drop and secondary oxidation; use an aluminum-carbon immersion nozzle from the middle ladle to the crystallizer to ensure verticality and centering, and the insertion depth of the immersion nozzle is 90±10 mm; use low-carbon acid-resistant steel protection slag for the crystallizer, and the protection slag must be dry and black-faced; use electromagnetic stirring during the production process; continuous casting cooling, the temperature before straightening is ≥900℃, ensure that the nozzle is not blocked, the water spray is uniform, and the position is centered to ensure the quality of the billet, and the surface is inspected and cleaned; S5: Heating: The temperature of the preheating section is ≤ 980°C. The heating temperature of the heating section and the soaking section is increased in the heating furnace. The furnace time is ≥ 120 min to ensure that the alloy elements V and Mo are fully and evenly dissolved in the austenite matrix. S6: Rolling: In the rolling process, micro-pile or micro-drawing rolling is adopted for rough rolling and intermediate rolling, and loop tension-free rolling is adopted for finishing rolling to avoid drawing steel rolling. Air cooling process is adopted after rolling to improve the strength of steel without sacrificing toughness, promote grain refinement, increase the yield strength and tensile strength of the material, improve the uniformity of the organization, and help to obtain a more uniform microstructure.

3. The production method of the chloride ion corrosion resistant hot-rolled ribbed steel bar MG500C for anchor rod according to claim 2 is characterized in that: The slag material in step S2 includes lime, dolomite and temperature regulating material, according to which lime accounts for 2 / 3 of the first batch, 1 / 3 of the later batch, all of dolomite, 3 / 4 of the temperature regulating material is added, and the rest is adjusted during "re-drying".

4. The production method of the chloride ion corrosion resistant hot-rolled ribbed steel bar MG500C for anchor rod according to any one of claims 2 or 3 is characterized in that: The soft argon blowing time in step S3 must not be less than 15 minutes.

5. The production method of the chloride ion corrosion resistant hot-rolled ribbed steel bar MG500C for anchor rod according to claim 4 is characterized in that: The continuous casting cooling in step S4 adopts a slow cooling mode.

6. The production method of the chloride ion corrosion resistant hot-rolled ribbed steel bar MG500C for anchor rod according to claim 5 is characterized in that: In step S5, the temperature of the heating section is controlled at 1140±20°C, and the temperature of the soaking section is controlled at 1160±20°C.

7. The production method of the chloride ion corrosion resistant hot-rolled ribbed steel bar MG500C for anchor rod according to claim 6 is characterized in that: In the step S6, the starting rolling temperature of the rough rolling is 1060±20°C, and the finishing rolling temperature is 940±20°C.

8. The method for producing the chloride ion corrosion resistant hot-rolled ribbed steel bar MG500C for anchor rod according to claim 7 is characterized in that: In step S6, pre-watering treatment is performed during the rolling process, and no watering is performed after rolling. The cooling rate of air cooling after rolling is controlled at 1-2°C / s.