Preparation method of (Cu, C) Ba2Can-1CunO2n+3 superconducting thin film applied to high-temperature superconducting filter

The high critical temperature (Cu,C)Ba2Can-1CunO2n+3 film was prepared on a single crystal substrate through pulsed laser deposition technology, which solved the problem of low critical temperature and preparation of existing high-temperature superconducting filter materials, and achieved high efficiency and low cost The high-temperature superconducting filter material preparation improves the anti-interference ability of the communication environment.

CN118910559AActive Publication Date: 2024-11-08NANJING UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410891768.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-11-08
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

The existing high-temperature superconducting filter materials have a low critical temperature, requiring liquid helium or liquid nitrogen to maintain a low temperature environment, resulting in high cost, limiting its commercial application, and preparing (Cu,C)Ba2Can- There are challenges in 1CunO2n+3 films.

Method used

(Cu,C)Ba2Can-1CunO2n+3 films were prepared on a single crystal substrate using pulsed laser deposition technology, and the film was chemically fired by barium, calcium and copper oxides or carbonates, and oxygen was introduced during the film growth process. and carbon dioxide, optimize laser energy, frequency, air pressure and substrate temperature to prepare superconducting films with high critical temperatures.

Benefits of technology

Successfully prepared (Cu,C)Ba2Ca2Cu3O9 and (Cu,C)Ba2Ca3Cu4O11 films with zero resistance transition temperature higher than YBCO. It has the advantages of non-toxic and green environmental protection, reduces the cost of use, and promotes the commercialization of high-temperature superconducting filters. application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910559A_ABST
    Figure CN118910559A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a (Cu, C) Ba2Can-1CannO2n + 3 superconducting thin film applied to a high-temperature superconducting filter, which comprises the following steps of: weighing a certain mass of oxides or carbonates of barium, calcium and copper according to a chemical proportion, and grinding, tabletting and sintering for multiple times to obtain a target material; mashing the obtained blocks in a mortar, and grinding the mashed blocks into uniform powder; putting the powder into a mold, and pressing into sheets; performing vacuum packaging by using a sealing bag, and further pressing in a hydraulic machine; after pressing, performing heat treatment in a heating furnace to obtain a PLD target material; polishing the prepared target material, and placing the target material in a PLD coating cavity; selecting a single crystal substrate with matched lattice constants; the preparation method comprises the following steps of: fixing the Cu, C) Ba2Can-1CannO2n + 3 thin film on a proper position of a base station, and then arranging the Cu, C) Ba2Can-1CannO2n + 3 thin film in a PLD (Pulsed Laser Deposition) coating cavity; the superconducting thin film with high critical temperature and low surface microwave impedance is obtained under proper laser energy, air pressure and substrate temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to (Cu,C)Ba2Ca for high temperature superconducting filter n-1 Cu n O 2n+3 (n=3,4) Superconducting film preparation method, applied to high-temperature superconducting weak current application field. Background Art

[0002] With the development of modern information technology, humans are becoming more and more dependent on electromagnetic wave transmission. From daily mobile communications to military, aerospace, radio astronomy and other scenarios, electromagnetic wave transmission is indispensable. With the advent of the 6G mobile communication era and the development of low-altitude satellites, more new microwave spectrum will be used. This also means that the radio spectrum will become more and more crowded, and the unused spectrum will become less and less. At the same time, the mutual interference between mobile communications, satellite communications, deep space exploration, etc. will become more and more serious. These will lead to more stringent requirements on the performance of microwave filters. Due to the limitation of microwave surface impedance, filters made of ordinary materials are difficult to meet the requirements of the rapidly developing communication environment.

[0003] In the microwave frequency range, the surface microwave resistance of superconducting materials below the critical temperature is less than one thousandth of that of normal metals. This also makes the filters made of superconducting films have the advantages of low loss, low noise, and high resonator Q value. Superconducting filters have great advantages in detecting weak signals, which can improve the anti-interference ability of wireless transmission and meet today's communication needs. For mobile communications, high-temperature superconducting filters can make mobile base stations cover a wider area under the same power consumption and improve communication quality. At present, the material used to prepare superconducting filters is mainly ReBCO, whose critical temperature is about 90K. The use of high-temperature superconducting filters requires the use of expensive mechanical refrigerators, which greatly limits the commercial application of superconducting filters. Increasing the ambient temperature of superconducting filters and reducing the cost of use will promote the application of superconducting filters and solve the problems faced by today's communication environment.

[0004] Conventional superconducting materials require liquid helium to maintain their low temperature environment due to their low critical temperature. Liquid helium is a non-renewable resource and is expensive, which greatly limits the application of superconducting materials. In 1986, scientists discovered copper oxide superconductors, and gradually discovered many high-temperature superconductors with superconducting transition temperatures higher than the boiling point of liquid nitrogen (77K, about minus 194°C). Due to its high critical temperature, it only needs liquid nitrogen to maintain its low temperature environment to appear in the superconducting state, which makes large-scale industrial applications possible. Copper oxide superconductors with superconducting transition temperatures higher than liquid nitrogen temperatures mainly include Y series, Bi series, Hg series and Tl series. Bi is currently mainly used in high-field environments in the liquid helium temperature zone. Hg series and Tl series copper oxide high-temperature superconductors are limited in application because they contain highly toxic elements. The critical temperature of the Y series (YBa2Cu3O7, referred to as YBCO) is around 90K, and it is the main material used in superconducting filters, but the cost of use is still too high.

[0005] In 1994, scientists discovered (Cu,C)Ba2Ca3Cu4O 11 , and its superconducting transition temperature is about 118K. Later, it was discovered that (Cu,C)Ba2Ca2Cu3O9 of the same system can reach a superconducting transition temperature of 120K after annealing after preparation. These two materials have high superconducting transition temperatures and are non-toxic and environmentally friendly. If high-performance thin film materials can be prepared and applied to microwave filters, their performance will be much better than YBCO because their superconducting transition temperature is much higher. The bulk materials of these materials are metastable and can currently only be synthesized under high temperature and high pressure. Due to the lattice mismatch between the lattice and the film, similar to the effect of physical pressure, the metastable material can be grown in the form of a thin film. But after more than 30 years of development, the preparation of (Cu,C)Ba2Ca n-1 Cu n O 2n+3 Thin films remain challenging. If (Cu,C)Ba2Ca with a higher critical temperature is prepared n-1 Cu n O 2n+3 Superconducting film may become a new type of material used in high-temperature superconducting filters, and reduce the cost of using high-temperature superconducting filters, enabling them to be more widely used commercially and solving the problems facing the current communication environment.

[0006] The applicant's research group has applied for a method to prepare (Cu,C)Ba2Ca on a metal soft substrate using pulsed laser deposition technology. n-1 Cu n O 2n+3 (n=3,4) thin film method. Application No. 2024104149184. Summary of the invention

[0007] In order to solve the existing technical problems, the purpose of the present invention is to provide a (Cu, C)Ba2Ca2O3 for high temperature superconducting filter prepared on a single crystal substrate by pulsed laser deposition technology. n-1 Cu n O 2n+3 (n=3,4) thin film method. Use barium, calcium and copper oxides or carbonates to sinter the target material in chemical proportion, and then use pulsed laser deposition technology to introduce oxygen and carbon dioxide during the film growth process to prepare a high critical temperature superconducting film, which has broad application prospects.

[0008] To achieve the above object, the present invention adopts the following technical scheme: preparing (Cu, C)Ba2Ca n-1 Cu n O 2n+3 (n=3,4) thin film method, comprising the following steps:

[0009] (1) Weigh a certain amount of barium, calcium and copper oxides or carbonates according to the ratio and mix them and grind them thoroughly, preferably for more than two hours to obtain a uniform powder; the preferred raw materials are BaCO3, CaCO3 and CuO; for (Cu,C)Ba2Ca3Cu4O 11 The optimal ratio of Cu in the target material used for preparation is 4.2-4.8; the optimal ratio of Cu in the target material used for preparation of (Cu,C)Ba2Ca2Cu3O9 is 3.2-3.8; 11 The target material used for the thin film can also adjust the conditions during the film growth to prepare (Cu,C)Ba2Ca2Cu3O9; the film growth conditions refer to laser energy, frequency, gas pressure, substrate, temperature, etc.

[0010] (2) placing the uniform powder ground in step (1) in a crucible or on a corundum sheet, placing it in a heating furnace, and heat treating the powder; controlling the heat treatment temperature to be 750-950° C., the heat treatment heating rate to be 1-10° C. / min, the heat treatment holding time to be 12-72 h, and the cooling rate to be 1-10° C. / min; preferably controlling the heat treatment temperature to be 800-860° C., the heat treatment heating rate to be 2-5° C. / min, the heat treatment holding time to be 24-48 h, and the cooling rate to be 2-5° C. / min;

[0011] (3) Grind the product fired in the above step into a uniform powder. Press the powder into a sheet by applying a pressure of 5-20MPa using a mold. Then take the block out of the mold, place it in a crucible with a stable bottom or on a corundum sheet, place it in a heating furnace, and perform heat treatment; control the heat treatment temperature to 750-950°C, the heat treatment heating rate to 1-10°C / min, the heat treatment constant temperature time to 12-72h, and the cooling rate to 1-10°C / min; preferably, the heat treatment temperature is 800-860°C, the heat treatment heating rate is 2-5°C / min, the heat treatment holding time is 24-48h, and the cooling rate is 2-5°C / min;

[0012] (4) Repeat step (3) 2-8 times.

[0013] (5) The block prepared in step (4) is fully ground to obtain a uniform powder. The powder is pressed into a tablet using a round mold, vacuum-sealed with a sealed bag, and then placed in a hydraulic press to press at a pressure of 40-100 Mba.

[0014] (6) Take the block pressed in step (5) out of the sealed bag and place it in a crucible with a stable bottom or on a corundum sheet. Place the crucible or corundum sheet in a heating furnace and heat treat the block to obtain the target material required for PLD coating; control the heat treatment temperature to 750-950°C, the heat treatment heating rate to 1-10°C / min, the heat treatment constant temperature time to 12-72h, and the cooling rate to 1-10°C / min; preferably control the heat treatment temperature to 800-860°C, the heat treatment heating rate to 2-5°C / min, the heat treatment constant temperature time to 24-60h, and the cooling rate to 2-5°C / min;

[0015] (7) Polishing the target material prepared in step (6) and then placing it in a PLD coating vacuum chamber.

[0016] (8) will be combined with (Cu,C)Ba2Ca n-1 Cu n O 2n+3 A single crystal substrate with a lattice constant matching the (n=3,4) material is fixed on a suitable position on a polished base and then installed in a PLD coating vacuum chamber; the single crystal substrates are LaAlO3, SrTiO3, YAlO3, LaMnO3, MgO, YSZ, NdCaAlO4, LaSrAlO4, LSAT, CeO2, NdGaO3, etc.; the position of the substrate on the base is directly opposite to the center of the feather glow.

[0017] (9) The base is heated to 600-800° C. The preferred temperature is 600-700° C. During this period, the vacuum environment in the PLD coating chamber is maintained.

[0018] (10) High-purity oxygen and carbon dioxide are introduced into the PLD coating chamber at a certain rate to maintain the gas pressure in the coating chamber at a constant value between 5 and 50 Pa. The ventilation scheme is that oxygen and carbon dioxide are introduced separately, and carbon dioxide flows toward the substrate; preferably, the oxygen flow rate is 20-30 sccm; preferably, the carbon dioxide flow rate is 3-10 sccm; and preferably, the gas pressure in the chamber is 10-30 Pa.

[0019] (11) Block the substrate with a baffle, turn on the laser, set the laser frequency to 2-10 Hz, and control the laser energy density to 0.5-8 J / cm 2 , perform pre-deposition for 2-15 minutes; the preferred laser energy density is 1.0-3.5 J / cm 2 , preferably the frequency is 5 Hz. During this period, the distance between the target and the substrate is adjusted so that the distance between the end of the plume and the substrate is 0.5-2.5 cm; preferably, the distance between the end of the plume and the substrate is about 1 cm.

[0020] (12) After the pre-deposition is completed, open the baffle to allow the substrate to dissipate heat for 2-10 minutes.

[0021] (13) Turn on the laser, set the energy to the same as the laser energy used in the pre-deposition in step (12), and the frequency to 2-10 Hz; and perform deposition. Preferably, the laser frequency is 5 Hz; and preferably, the deposition time is 20-40 minutes.

[0022] (14) After the deposition is completed, if in-situ annealing is used, oxygen or nitrogen must be introduced into the PLD coating chamber to maintain the pressure in the chamber at 10 1 -10 5 Pa; the cooling rate of the temperature from the deposition temperature to the in-situ annealing temperature is 1-10°C / min; the in-situ annealing temperature is 300-650°C; the in-situ annealing time is 0-3h; the cooling rate of the temperature from the in-situ annealing temperature to room temperature is 1-10°C / min; the annealing scheme is preferably in-situ annealing. The preferred annealing dwell temperature is 450-550°C, the preferred annealing gas is oxygen, and the preferred heating and cooling rate is 5-8°C / min.

[0023] (15) If ex-situ annealing is adopted, the temperature of the substrate is lowered from the deposition temperature to room temperature at a cooling rate of 1-10°C / min; the prepared film is placed in an atmosphere heating furnace for oxygen or nitrogen annealing. The preferred annealing dwell temperature is 450-550°C; the heating and cooling rate is 5-8°C / min. Under appropriate laser energy, gas pressure and substrate temperature, a superconducting film with high critical temperature and low surface microwave impedance is obtained.

[0024] Beneficial effects: Compared with the prior art, the present invention has the following obvious outstanding substantive features and significant advantages:

[0025] 1. The method of the present invention prepares a c-axis oriented (Cu, C) Ba2Ca2Cu3O9 thin film on a single crystal substrate by optimizing the film preparation conditions and adjusting the position and angle of carbon dioxide and oxygen inlet. This has not been reported before. Its zero resistance transition temperature is 98K, which is higher than the superconducting transition temperature of YBCO. Based on the understanding of the properties of (Cu, C) Ba2Ca2Cu3O9 bulk material, the critical temperature can be further improved.

[0026] 2. The method of the present invention optimizes the film preparation conditions and adjusts the position and angle of carbon dioxide and oxygen inlet through pulsed laser deposition technology to prepare (Cu, C)Ba2Ca3Cu4O with a zero resistance transition temperature higher than 96K on a single crystal substrate. 11 The film has an initial transition temperature of 117 K. After optimizing the conditions, the zero resistance transition temperature can be further increased.

[0027] 3. (Cu,C)Ba2Ca n-1 Cu n O 2n+3 (n=3,4)Superconducting materials have advantages such as non-toxicity and high critical temperature. Successful preparation of thin film materials on single crystal substrates and preparation of microwave filters will reduce their use costs and promote their commercial use, which will have broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a RT relationship diagram of the (Cu, C)Ba2Ca2Cu3O9 film prepared in Example 1 of the present invention.

[0029] Figure 2 This is a RT relationship diagram of the (Cu, C)Ba2Ca2Cu3O9 film prepared in Example 2 of the present invention.

[0030] Figure 3 The (Cu,C)Ba2Ca3Cu4O prepared in Example 3 of the present invention 11 RT plot of the film.

[0031] Figure 4 The (Cu,C)Ba2Ca3Cu4O prepared in Example 3 of the present invention 11 XRD diffraction pattern of the film. DETAILED DESCRIPTION

[0032] The above scheme is further described below in conjunction with specific implementation examples. The preferred embodiments of the present invention are described in detail as follows:

[0033] Embodiment 1: A method for preparing a (Cu, C)Ba2Ca2Cu3O9 thin film on a SrTiO3 single crystal substrate, comprising the following steps:

[0034] (1) According to Ba2Ca3Cu 4.6 O y A certain mass of high-purity BaCO3, CaCO3 and CuO powders are weighed according to the chemical proportion, mixed and ground into a uniform powder in a mortar with powder particles less than 10 microns; the uniformly ground powder is placed in a crucible or on a corundum sheet, put into a heating furnace, and heat treated in air; the heat treatment temperature is 800°C, and the heat treatment constant temperature time is 24h; BaO and CaO can also be selected to replace BaCO3 and CaCO3 respectively.

[0035] (2) Grind the product obtained in the above step again to obtain a uniform powder. Press the powder into a sheet with a mold under a pressure of 10 MPa, and put it into a heating furnace for heat treatment; the heat treatment temperature is 830°C or other temperatures within the above heating range, and the heat treatment holding time is 24 hours. Repeat this step 2-8 times. The pressure can be 5 MPa or 15 MPa.

[0036] (3) Grind the block obtained in step (2) into uniform powder, and press it into a sheet with a pressure of 10 MPa using a mold. Then seal it with a vacuum bag, place it in a hydraulic press, and press it with a pressure of 66 MPa (50 or 100 MPa is also acceptable). Take out the block and place it in a heating furnace for heat treatment. The heat treatment temperature is 860°C, and the heat treatment holding time is 48 hours; the above heat treatment heating and cooling rates are all 5°C / min;

[0037] The heat treatment temperature can be 800℃-900℃; the heat treatment holding time can be 24-48h, or 72h; the heat treatment heating rate can be 1-10℃ / min, and the cooling rate can be 1-10℃ / min, and basically the same results can be obtained.

[0038] (4) polishing the target material prepared in step (3), and then placing it in a PLD coating vacuum chamber; fixing the single crystal substrate at a position where the base is facing the laser plume, and then placing it in the PLD coating vacuum chamber;

[0039] (5) Heat the substrate to 640°C. During this period, the vacuum environment in the PLD coating chamber is maintained. After the temperature stabilizes, high-purity oxygen and carbon dioxide are introduced into the PLD coating chamber from different inlets. Oxygen is introduced at a rate of 30 sccm, and carbon dioxide is introduced at a rate of 5 sccm, maintaining the pressure in the coating chamber at 20 Pa. The volume of carbon dioxide is generally 5%-25% of that of oxygen.

[0040] (6) Block the substrate with a baffle and turn on the laser. The laser energy density is 1 to 3 J / cm 2 , the frequency is 5Hz, and the pre-deposition can be carried out for 5mins; the distance between the target and the substrate is adjusted to 4cm. After the pre-deposition is completed and the temperature is stable, the film is deposited for 20mins, and the laser energy and frequency remain unchanged. The single crystal substrates used for the substrate are LaAlO3, SrTiO3, YAlO3, LaMnO3, NdCaAlO4, LaSrAlO4, LSAT, CeO2, and NdGaO3, all of which have grown superconducting films. It can also be grown on substrates with LaMnO2 and CeO2 as cap layers.

[0041] (7) After the deposition is completed, the pressure in the PLD coating chamber is maintained during the film deposition, and the temperature is lowered to room temperature at a rate of 5°C / min. Oxygen or nitrogen can also be introduced to perform in-situ annealing to adjust the oxygen content.

[0042] Experimental test analysis of this embodiment:

[0043] The (Cu,C)Ba2Ca2Cu3O9 thin film prepared in this example was characterized and measured by using a comprehensive physical property measurement system (PPMS) to measure the resistance-temperature curve of the thin film. Figure 1 The relationship between the resistivity of the film and the temperature is shown in Figure 2. It can be seen that the zero resistance temperature of the film is about 98K. Taking 90% of the normal resistance as the standard, the initial transition temperature is It is about 110K.

[0044] This experiment prepared a C-oriented (Cu, C) Ba2Ca2Cu3O9 film for the first time, and its transition temperature is higher than the maximum reported transition temperature of (Cu, C) Ba2Cu3O9 film. It is also higher than the highest transition temperature of YBCO. This material will have a wide range of application prospects. According to the research report on its bulk material, its oxygen content can be adjusted by different annealing conditions, thereby further increasing its superconducting transition temperature.

[0045] Embodiment 2: A method for preparing a (Cu, C)Ba2Ca2Cu3O9 thin film on a LSAT single crystal substrate, comprising the following steps:

[0046] (1) The target material preparation method is the same as that in Example 1.

[0047] (2) The substrate is fixed on a base platform facing the laser plume, dried, and then placed in a PLD coating vacuum chamber;

[0048] (3) The substrate is heated to 620° C. After the temperature stabilizes, high-purity oxygen and carbon dioxide are introduced into the PLD coating chamber, with oxygen introduced at a rate of 30 sccm and carbon dioxide flowing to the substrate at a rate of 5 sccm, maintaining the gas pressure in the coating chamber at 20 Pa.

[0049] (4) Adjust the laser energy density to 1-2 J / cm 2 , the frequency is 5Hz. Pre-deposition target washing is carried out for 5 minutes to remove pollutants attached to the surface; after the pre-deposition is completed and the temperature is stabilized, thin film deposition is carried out, the deposition time is 20 minutes, and the laser energy and frequency remain unchanged.

[0050] (5) After the deposition is completed, high-purity oxygen is introduced into the PLD coating chamber to maintain the pressure in the chamber at 7×10 4 The temperature was lowered to 500°C at a rate of 5°C / min and kept for 1 hour for in-situ annealing; then the temperature was lowered to room temperature at a rate of 5°C / min.

[0051] Experimental test analysis of this embodiment: The (Cu, C)Ba2Ca2Cu3O9 film prepared in this embodiment was characterized, and the resistance of the film was measured using a comprehensive physical property measurement system (PPMS). Figure 2 This is the relationship curve of the resistivity of the film with temperature. As shown in the figure, the zero resistance temperature of the film is about 92K. Taking 90% of the normal resistance as the standard, its initial transformation temperature The film is c-oriented according to X-ray diffraction analysis. This example is the first to prepare a (Cu,C)Ba2Ca2Cu3O9 film on an LSAT substrate, and its critical temperature is similar to that of the materials currently used in filters. Changing the annealing conditions or further optimizing the preparation conditions can further increase its superconducting transition temperature.

[0052] Example 3: Preparation of (Cu,C)Ba2Ca3Cu4O on YAlO3 single crystal substrate 11 The method for preparing the film comprises the following steps:

[0053] (1) The target material preparation method is the same as that in Example 1.

[0054] (2) The substrate is fixed on a base platform facing the laser plume, dried on a heating platform, and then placed in a PLD coating vacuum chamber;

[0055] (3) The substrate is heated to 665° C. After the temperature stabilizes, high-purity oxygen and carbon dioxide are introduced into the PLD coating chamber, with oxygen introduced at a rate of 30 sccm and carbon dioxide flowing to the substrate at a rate of 5 sccm, maintaining the gas pressure in the coating chamber at 20 Pa.

[0056] (4) Adjust the laser energy density to 1-3 J / cm 2 , frequency is 5Hz, and pre-deposition is carried out for 5 minutes; after the pre-deposition is completed and the temperature is stable, the thin film is deposited for 20 minutes, and the laser energy and frequency remain unchanged.

[0057] (5) After the deposition is completed, high-purity oxygen is introduced into the PLD coating chamber to maintain the pressure in the chamber at 5×10 4 The temperature was lowered to 500°C at a rate of 5°C / min and kept for 1 hour for in-situ annealing; then the temperature was lowered to room temperature at a rate of 5°C / min.

[0058] Experimental test analysis of this embodiment:

[0059] In this example, (Cu,C)Ba2Ca3Cu4O 11 The film was characterized and the RT curve of the film was measured using a comprehensive physical property measurement system (PPMS). Figure 3 This is the relationship curve of the resistivity of the film with temperature. As shown in the figure, the zero resistance temperature of the film is about 96K. Taking 90% of the normal resistance as the standard, its initial transformation temperature It is 117K. Figure 4 is the X-ray diffraction spectrum of the film, showing the (h00) diffraction peak of the film, indicating that the film is a-oriented. This example is the first to prepare (Cu,C)Ba2Ca3Cu4O on a YAO substrate. 11 The critical temperature of the film is higher than that of the materials currently used in filters. After the film is grown, it is annealed in high-purity oxygen to reduce the defects and oxygen deficiency that may occur in the film during the growth process.

[0060] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Without departing from the purpose and spirit of the claims of the present invention, any method for preparing a (Cu, C)Ba2Ca2O3 for a superconducting filter on a single crystal substrate is n-1 Cu n O 2n+3 Various changes such as changes and modifications of the method for making (n=3, 4) superconducting thin films all fall within the protection scope of the present invention.

Claims

1. A (Cu,C)Ba2Ca for high temperature superconducting filter applications n-1 Cu n O 2n+3 (n=3,4) A method for preparing a superconducting thin film, characterized in that: (1) weighing a certain amount of oxides or carbonates of barium, calcium and copper according to a chemical ratio, mixing and grinding into a uniform powder; then placing in a heating furnace for heat treatment; grinding the prepared product several times into a uniform powder, pressing into a tablet, and placing in a heating furnace for heat treatment; (2) placing the block obtained in step (1) in a mortar, crushing and grinding it into a uniform powder; placing the powder in a mold and pressing it into a sheet; then vacuum-packing it in a sealed bag, placing it in a hydraulic press for further pressing; placing it in a heating furnace for heat treatment after pressing to obtain a PLD target; polishing the prepared target and placing it in a PLD coating chamber; (3) Select (Cu,C)Ba2Ca n-1 Cu n O 2n+3 (n=3,4) a single crystal substrate with a matching lattice constant; fix it on a suitable position on a base, then install it in a PLD coating chamber, and maintain the vacuum of the chamber for heating; in step (3), the single crystal substrate used is LaAlO3, SrTiO3, YAlO3, MgO, LaMnO3, YSZ, NdCaAlO4, LaSrAlO4, LSAT, CeO2, NdGaO3, etc.; (4) After the temperature reaches the specified temperature, high-purity oxygen and carbon dioxide are introduced into the PLD coating chamber at a certain flow rate to maintain a constant air pressure in the coating chamber; (5) Adjust the distance between the target and the substrate so that the distance between the end of the plume and the substrate is appropriate; after the temperature stabilizes, the thin film is deposited and grown; (6) After the deposition is completed, the air pressure is maintained in the PLD coating chamber, or oxygen or nitrogen is introduced to perform in-situ annealing; or the air pressure is directly reduced to room temperature, and the sample is placed in a ventilation heating furnace for ex-situ annealing; According to the ratio, weigh a certain amount of barium, calcium and copper oxides or carbonates, mix them and grind them thoroughly, preferably for more than two hours to obtain a uniform powder; the preferred raw materials are BaCO3, CaCO3 and CuO; for (Cu,C)Ba2Ca3Cu4O 11 The target material used in the preparation has a Cu ratio of 4.2-4.8; the target material used in the preparation of (Cu, C) Ba2Ca2Cu3O9 has a Cu ratio of 3.2-3.8; the target material used in the preparation of (Cu, C) Ba2Ca3Cu4O 11 The target material used for the thin film adjusts the conditions during the film growth to prepare (Cu,C)Ba2Ca2Cu3O9; the film growth conditions refer to laser energy, frequency, gas pressure, substrate, and temperature.

2. The method for preparing a superconducting thin film according to claim 1, characterized in that: The specific steps are as follows: (1) weighing a certain mass of oxides or carbonates of barium, calcium and copper according to a chemical ratio, mixing and grinding the mixture into a uniform powder; (2) placing the uniform powder ground in the step (1) in a crucible or on a corundum sheet, placing the mixture in a heating furnace, and subjecting the powder to heat treatment; controlling the heat treatment temperature to 750-950°C, the heat treatment heating rate to 1-10°C / min, the heat treatment holding time to 12-72h, and the cooling rate to 1-10°C / min; preferably controlling the heat treatment temperature to 800-860°C, the heat treatment heating rate to 2-5°C / min, the heat treatment holding time to 24-48h, and the cooling rate to 2-5°C / min; Step (3) grinding the product fired in the above step into a uniform powder; pressing the powder into a sheet by applying a pressure of 5-20 MPa using a mold; then taking the block out of the mold, placing it in a crucible with a stable bottom or on a corundum sheet, placing it in a heating furnace, and performing heat treatment; controlling the heat treatment temperature to be 750-950° C., the heat treatment heating rate to be 1-10° C. / min, the heat treatment constant temperature time to be 12-72 h, and the cooling rate to be 1-10° C. / min; preferably, the heat treatment temperature is 800-860° C., the heat treatment heating rate to be 2-5° C. / min, the heat treatment holding time to be 24-48 h, and the cooling rate to be 2-5° C. / min; Step (4) repeating step (3) 2-8 times; Step (5) fully grinding the block prepared in step (4) to obtain a uniform powder; pressing the powder into a tablet using a round mold, vacuum-sealing it with a sealed bag, placing it in a hydraulic press, and pressing it at a pressure of 40-100 Mba; Step (6) taking the block pressed in step (5) out of the sealed bag and placing it in a crucible with a stable bottom or on a corundum sheet; placing the crucible or the corundum sheet in a heating furnace, and heat treating the block to obtain the target material required for PLD coating; controlling the heat treatment temperature to 750-950°C, the heat treatment heating rate to 1-10°C / min, the heat treatment constant temperature time to 12-72h, and the cooling rate to 1-10°C / min; preferably controlling the heat treatment temperature to 800-860°C, the heat treatment heating rate to 2-5°C / min, the heat treatment constant temperature time to 24-60h, and the cooling rate to 2-5°C / min; Step (7) polishing the target material prepared in step (6) and then placing it in a PLD coating vacuum chamber; Step (8) will be with (Cu,C)Ba2Ca n-1 Cu n O 2n+3 A single crystal substrate with a lattice constant matching that of the (n=3,4) material is fixed on a suitable position of a polished base and then installed in a PLD coating vacuum chamber; the single crystal substrate is LaAlO3, SrTiO3, YAlO3, LaMnO3, MgO, YSZ, NdCaAlO4, LaSrAlO4, LSAT, CeO2 or NdGaO3; the position of the substrate on the base is directly opposite to the center of the feather glow; Step (9) heating the base to 600-800° C.; preferably 600-700° C.; during which the vacuum environment in the PLD coating chamber is maintained; Step (10) high-purity oxygen and carbon dioxide are introduced into the PLD coating chamber at a certain rate to maintain the pressure in the coating chamber at a constant value between 5-50 Pa; the ventilation scheme is that oxygen and carbon dioxide are introduced separately, and carbon dioxide flows toward the substrate; the oxygen flow rate is 20-30 sccm; the carbon dioxide flow rate is preferably 3-10 sccm; the pressure in the chamber is 10-30 Pa; Step (11) Block the substrate with a baffle, turn on the laser, set the laser frequency to 2-10 Hz, and control the laser energy density to 0.5-8 J / cm 2 , pre-deposition for 2-15 minutes; laser energy density is 1.0~3.5J / cm 2 , the frequency is 2-10Hz; during this period, the distance between the target and the substrate is adjusted so that the distance between the end of the plume and the substrate is 0.5-2.5cm; preferably, the distance between the end of the plume and the substrate is about 1cm; After the pre-deposition in step (12) is completed, the baffle is opened to allow the substrate to dissipate heat for 2-10 minutes; Step (13) turning on the laser, setting the energy to be the same as the laser energy used for pre-deposition in step (12), and the frequency to be 2-10 Hz; performing deposition; preferably the laser frequency is 5 Hz; and preferably the deposition time is 20-40 minutes; Step (14) After the deposition is completed, if in-situ annealing is adopted, oxygen or nitrogen needs to be introduced into the PLD coating chamber to maintain the pressure in the chamber at 10 1 -10 5 Pa; the cooling rate of the temperature from the deposition temperature to the in-situ annealing temperature is 1-10°C / min; the in-situ annealing temperature is 300-650°C; the in-situ annealing time is 0-3h; the cooling rate of the temperature from the in-situ annealing temperature to room temperature is 1-10°C / min; the annealing scheme is preferably in-situ annealing; The annealing dwell temperature is 450-550℃, the annealing gas is oxygen, and the heating and cooling rate is 5-8℃ / min; Step (15) If ex-situ annealing is adopted, the temperature of the base is lowered from the deposition temperature to room temperature at a cooling rate of 1-10°C / min; the prepared film is placed in an atmosphere heating furnace for oxygen or nitrogen annealing treatment; The annealing dwell temperature is selected to be 450-550°C; the heating and cooling rate is 5-8°C / min.

3. The preparation method according to claim 2, characterized in that: In the step (1), the raw materials used are high-purity BaCO3 or BaO, CaCO3 or CaO, CuO; for (Cu, C)Ba2Ca3Cu4O 11 The target material used in the preparation has a Cu ratio of 4.2-4.8; the target material used in the preparation of (Cu, C) Ba2Ca2Cu3O9 has a Cu ratio of 3.2-3.8; the target material used in the preparation of (Cu, C) Ba2Ca3Cu4O 11 By adjusting the growth conditions of the thin film, the target material used for the thin film can also prepare (Cu,C)Ba2Ca2Cu3O9.

4. The preparation method according to claim 1, characterized in that: In the steps (1) and (2), the heat treatment temperature is 750-950°C; the heat treatment heating rate is 1-10°C / min, the heat treatment constant temperature time is 12-72h, and the cooling rate is 1-10°C / min.

5. The preparation method according to claim 1 or 2, characterized in that: In the step (5), when the target material is pressed by a hydraulic press, the pressure is 40-100 Mba.

6. The preparation method according to claim 2, characterized in that: In the step (10), the ventilation scheme is that oxygen and carbon dioxide are introduced separately; oxygen enters the coating chamber at a rate of 10-50sccm; carbon dioxide enters the coating chamber at a rate of 1-30sccm and flows toward the substrate; the air pressure in the coating chamber is 5-50Pa.

7. The preparation method according to claim 2, characterized in that: In step (13), the temperature of the base in the cavity is 600-800°C, and the laser energy density is 0.5-8 J / cm 2 ; The laser frequency is 2-10 Hz; The distance between the end of the plume and the single crystal substrate is 0.5-2.5 cm.

8. The preparation method according to claim 2, characterized in that:In step (14), if in-situ annealing is adopted, oxygen or nitrogen needs to be introduced into the PLD coating chamber so that the pressure in the chamber is maintained at 10 1 -10 5 Pa; the temperature is reduced from the deposition temperature to the in-situ annealing temperature at a cooling rate of 1-10°C / min; the in-situ annealing dwell temperature is 350-650°C; the in-situ annealing dwell time is 0-3h; the temperature is reduced from the in-situ annealing temperature to room temperature at a cooling rate of 1-10°C / min; if ex-situ annealing is adopted, the temperature is reduced from the deposition temperature to room temperature at a cooling rate of 1-10°C / min; the prepared film is placed in a ventilation heating furnace for annealing treatment with oxygen or nitrogen; the annealing dwell temperature is 300-650°C; the annealing dwell time is 0-3h; the heating and cooling rate is 1-10°C / min.

9. The preparation method according to claim 8, characterized in that: The oxygen content of the prepared film varies with the annealing conditions.

Citation Information

Patent Citations

  • Ba-Ca-Cu-O compositions superconducting at up to 126 K and methods for making same

    CN1240414A

  • Oxide superconductive thin film

    JP2013095648A