Preparation method of non-uniform optical material surface reflection low-loss film system
By vacuum plating the reflective low-loss film system on the surface of non-uniform optical materials, using silica, tantalum pentoxide and mask plate technology, the problem of high reflectivity of non-uniform optical materials is solved, and low loss is achieved and efficient signal transmission.
Patent Information
- Application Number
- CN202410972666.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
The surface reflectivity of non-uniform optical materials is relatively high, which affects the signal-to-noise ratio, stray light and imaging contrast of integrated devices, and cannot meet the signal transmission requirements of high, precise and sharp integrated optoelectronic devices.
Vacuum plating of reflective low-loss film system on the surface of non-uniform optical materials. By determining the refractive index distribution formula of the optical material, selecting silica and tantalum pentoxide as film-based materials, designing the film-based thickness, and calculating the film-based combination with air The optical admittance distribution is used to adjust the film thickness using the mask plate, and the film system is prepared by ion beam sputtering vacuum coating technology.
It realizes ultra-low reflection loss at the spectral wavelength energy used, improves the signal-to-noise ratio and imaging contrast of integrated devices, and meets the signal transmission requirements of high, precise and sharp integrated optoelectronic devices.
Smart Images

Figure CN118910560A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optical film preparation, and in particular relates to a method for preparing a non-uniform optical material surface reflective low-loss film system. Background Art
[0002] Inhomogeneous materials mainly refer to some special new optical materials such as optical plastics, optical crystals, composite optical glass, doped optical materials, etc. whose refractive index changes linearly or nonlinearly in the spectral transparent region. With the development of science and technology, this new type of optical material is increasingly being widely used in aerospace information detection, integrated optoelectronic chips, advanced medical imaging and other industries.
[0003] However, the surface reflectivity of non-uniform optical materials is relatively high, and their performance affects the signal-to-noise ratio, stray light, imaging contrast, etc. of integrated devices, and there is a problem that they cannot meet the requirements of signal transmission in high-precision and cutting-edge integrated optoelectronic devices. For this reason, the field urgently needs to develop a method for preparing a low-loss film system for the surface reflection of non-uniform optical materials to achieve ultra-low reflection loss of non-uniform optical materials in the utilized spectral wavelength energy. Summary of the invention
[0004] The purpose of the present invention is to solve the above-mentioned technical problems and to propose a method for preparing a reflective low-loss film system on the surface of a non-uniform optical material. By vacuum-plating a reflective low-loss film system on the surface of a non-uniform optical material, ultra-low reflection loss of the energy of the utilized spectral wavelength can be achieved, so as to specifically solve the problem that the reflectivity of the surface of the non-uniform optical material is relatively high, and its performance affects the signal-to-noise ratio, stray light, imaging contrast, etc. of the integrated device, and cannot meet the requirements of signal transmission in high-precision and cutting-edge integrated optoelectronic devices.
[0005] The technical solution proposed in this application is: a method for preparing a low-loss film system with surface reflection on a non-uniform optical material, comprising the following steps:
[0006] S1. Determine the refractive index distribution formula of optical materials;
[0007] S2. Select membrane materials;
[0008] S3. Design the film thickness;
[0009] S4. Calculate the optical admittance distribution of the film system and air combination at different wavelengths;
[0010] S5. Calculate the size of the mask plate;
[0011] S6, preparing a membrane system;
[0012] S7. Determine the film spectrum curve.
[0013] Preferably, in step S1, assuming that the optical material is a rectangular structure with non-uniform longitudinal distribution, with a longitudinal dimension from a to b and a transverse dimension from c to d, the formula for the non-uniform longitudinal distribution of the refractive index of the optical material is as follows:
[0014] n=f 1 (x), a≤x≤b;
[0015] If the optical material is a special-shaped part, the special-shaped part is enclosed by a rectangular structure, and the size of the special-shaped part is equivalent to the size of the rectangular structure.
[0016] Preferably, in step S2, silicon dioxide and tantalum pentoxide are selected as film materials. Silicon dioxide and tantalum pentoxide are selected as film materials. There are many kinds of optical film materials, such as silicon dioxide (SiO2), aluminum oxide (Al2O3), tantalum pentoxide (Ta2O5), titanium dioxide (TiO2), etc. The present application selects silicon dioxide and tantalum pentoxide as two film materials for preparation. This is because these two film materials are both oxides, have high chemical stability, good mechanical strength, and strong bonding between the film material and the non-uniform optical material substrate. Preparation on the surface of the non-uniform optical material substrate is conducive to improving the overall acid resistance, alkali resistance and environmental adaptability of the non-uniform optical material.
[0017] Preferably, step S3 includes the following steps:
[0018] S31, select the center of the longitudinal position of the optical material, whose refractive index is n g , at the corresponding wavelength λ 0 , the reflectivity of the designed film system is zero, where:
[0019] n g =f(x g ), x g =(a+b) / 2;
[0020] S32. The optical material is optical glass, and is used as a substrate for film system design. The refractive index of the corresponding film layer in the film system is as follows:
[0021] Refractive index of silicon dioxide: η 1 =n SiO2 ;
[0022] Tantalum pentoxide refractive index: η 2 =n Ta2O5 ;
[0023] Substrate refractive index: η g =n glass ;
[0024] Refractive index of air: η a =n air ;
[0025] S33, corresponding wavelength λ 0 , calculate the phase thickness of the corresponding film layer under the corresponding physical thickness according to the film phase thickness formula:
[0026] Assume that the physical thickness of the first silicon dioxide film is d 1 , its phase thickness is:
[0027] Assume that the physical thickness of the second tantalum pentoxide film is d 2 , its phase thickness is:
[0028] Then the characteristic matrix of the film system is obtained as follows:
[0029] The first layer of silicon dioxide film features matrix:
[0030]
[0031] The second layer of tantalum pentoxide film characteristic matrix:
[0032]
[0033] The matrix formula of the film system and optical glass combination characteristics is as follows:
[0034]
[0035] Corresponding wavelength λ 0 , the calculation formula of the film reflectivity is as follows:
[0036]
[0037] S34, substituting the corresponding wavelength data into step S33, the physical thickness of each film layer when the reflectivity of the film system is zero can be obtained.
[0038] Preferably, in step S4, at different wavelengths, the calculation formula for the optical admittance distribution of the film system combined with air is as follows:
[0039]
[0040] Y=F / E=N-iK=f 2 (λ).
[0041] Preferably, in step S5, when the refractive index of the substrate and the optical admittance of the film system combined with air are approximately equal, the reflectivity of the film system is approximately zero, and the corresponding relationship between the wavelength and the refractive index distribution of the substrate is as follows:
[0042] n=f 1 (x)≈Y=f 2 (λ);
[0043] f 1 (x)≈f 2 (λ0;
[0044] have to:
[0045] λ≈f 3 (x), a≤x≤b;
[0046] According to the film phase thickness formula in step S33, it can be known that when the film thickness changes in proportion to the wavelength, the reflectivity result of the film is not affected. Therefore, the preparation thickness of the film material at different positions of the refractive index on the substrate surface is changed through the mask plate, and the zero reflectivity wavelengths at different positions of the film material are overlapped, that is, the ultra-low reflection loss of the entire substrate surface after coating is obtained, which is approximately zero;
[0047] When there is no mask in front of the substrate, the refractive index n of the longitudinal center of the substrate g At wavelength λ 0 is the zero reflectivity wavelength; when a mask is installed in front of the substrate and the overall width of the mask is ω, the refractive index n at the center of the longitudinal position of the substrate g At wavelength λ′ 0 is the new zero reflectivity wavelength; then the mask width is corrected to:
[0048]
[0049] And (dc) / 10≤ω≤(dc) / 4.
[0050] Preferably, in step S6, ion beam sputtering and auxiliary methods are selected for vacuum coating. During the vacuum coating process, a mask plate is placed in front of the substrate to change the film thickness distribution on the substrate surface so that the film thickness gradually changes on the surface of the substrate to prepare a film system.
[0051] Preferably, in step S6, vacuum coating is performed using a dual ion beam sputtering coating machine, and the process includes the following steps:
[0052] S61, perform substrate surface quality inspection to ensure that there is no deteriorated layer, broken points or scratches on the substrate surface;
[0053] S62, using absorbent gauze dipped in a 1:1 alcohol-ether mixture by volume ratio to clean the substrate, and using a breath method to check the cleanliness of the substrate. If the surface of the substrate is evenly covered with air after the breath, it is clean. If the surface is unevenly covered with air or there are spots, further wipe it. After cleaning, load the substrate into a dual ion beam sputtering coating machine, and install a mask plate in front of the substrate;
[0054] S63, vacuuming, when the vacuum degree of the dual ion beam sputtering coating machine reaches 6×10 -2 Pa~9×10 -2When the temperature is Pa, the substrate is baked at 100℃~120℃ and kept at a constant temperature for 30min~40min to improve the firmness of the film;
[0055] S64, continue to evacuate, when the vacuum degree is 2×10 -3 Pa~3×10 -3 When the pressure is 0.0457 W / m2, the argon flow rate of the 12 cm RF radio frequency auxiliary ion source is adjusted to 3 sccm, the oxygen flow rate is adjusted to 25 sccm, the argon flow rate of the neutralizer is adjusted to 5 sccm, the beam intensity is adjusted to 200 mA, and the substrate surface is cleaned for 5 min to 10 min to remove dust, water stains and oil stains on the substrate surface;
[0056] S65, after cleaning, adjust the argon flow rate of the 16cm RF sputtering ion source to 18sccm, the beam intensity to 600mA, adjust the argon flow rate of the 12cm RF auxiliary ion source to 3sccm, the oxygen flow rate to 25sccm, the argon flow rate of the neutralizer to 5sccm, the beam intensity to 200mA, and deposit the first tantalum pentoxide film at a rate of 0.24nm / s to a designed thickness, and then deposit the second silicon dioxide film at a rate of 0.22nm / s to a designed thickness;
[0057] S66, turn off the ion source of the dual ion beam sputtering coater and cool the equipment.
[0058] Preferably, in step S7, the spectral characteristics of the entire substrate surface after coating are measured using a spectrophotometer, and it is measured that the reflectivity of the entire substrate surface after coating at the required wavelength is close to zero.
[0059] Preferably, the dual ion beam sputtering coating machine adopts the American Veeco dual ion beam sputtering coating machine.
[0060] The present invention also includes other steps or devices that can enable the normal use of a method for preparing a non-uniform optical material surface reflective low-loss film system, all of which are conventional means in the field. In addition, steps or devices not limited in the present invention all adopt the existing technology in the field.
[0061] The beneficial effects of the present invention are: it has the advantages of simple process, convenient operation and easy promotion, and by vacuum-plating a reflective low-loss film system on the surface of a non-uniform optical material, an ultra-low reflection loss of the energy of the utilized spectral wavelength is achieved, thereby specifically solving the problem that the reflectivity of the surface of the non-uniform optical material is relatively high, and its performance affects the signal-to-noise ratio, stray light, imaging contrast, etc. of the integrated device, and cannot meet the requirements for signal transmission in high-precision and cutting-edge integrated optoelectronic devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 Graph showing longitudinal size distribution of the non-uniform optical material in the embodiment.
[0063] Figure 2 Graph showing the equivalent optical admittance distribution of the film system combined with air at different wavelengths in the embodiment.
[0064] Figure 3 Schematic diagram of the dimensions of the mask plate in the embodiment.
[0065] Figure 4 Schematic diagram of ion beam sputtering and auxiliary coating method in the embodiment.
[0066] Figure 5 It is the spectral characteristic curve of the film system in the embodiment.
[0067] Figure 6 It is a gradient diagram of the film thickness distribution on the substrate surface in the embodiment.
[0068] Figure 7 It is a graph of the actual measured spectrum of the film system on the substrate surface in a specific application in the embodiment. DETAILED DESCRIPTION
[0069] The technology of the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.
[0070] Example
[0071] like Figures 1 to 6 As shown, this embodiment proposes a method for preparing a low-loss film system on the surface of a non-uniform optical material, comprising the following steps:
[0072] S1. Determine the refractive index distribution formula of optical materials;
[0073] like Figure 1 As shown, assuming that the optical material is a rectangular structure with non-uniform longitudinal distribution, the longitudinal dimension is from a to b, and the transverse dimension is from c to d, then the formula for the non-uniform longitudinal distribution of the refractive index of the optical material is as follows:
[0074] n=f 1 (x), a≤x≤b;
[0075] If the optical material is a special-shaped part, the special-shaped part is enclosed by a rectangular structure, and the size of the special-shaped part is equivalent to the size of the rectangular structure.
[0076] It should be noted that Figure 1 In the figure, the horizontal axis is the position and the vertical axis is the refractive index.
[0077] S2. Select membrane materials;
[0078] Silicon dioxide and tantalum pentoxide are selected as film materials. There are many kinds of optical film materials, such as silicon dioxide (SiO 2 ), aluminum oxide (Al 2 O3 ), Tantalum pentoxide (Ta 2 O 5 ), titanium dioxide (TiO 2 ) etc. In this embodiment, two kinds of film materials, silicon dioxide and tantalum pentoxide, are selected for preparation. This is because these two film materials are both oxides, have the advantages of high chemical stability, good mechanical strength, and strong bonding between the film materials and the non-uniform optical material substrate. Preparation on the surface of the non-uniform optical material substrate is conducive to improving the overall acid resistance, alkali resistance and environmental adaptability of the non-uniform optical material.
[0079] S3. Design the film thickness, including the following steps:
[0080] S31, select the center of the longitudinal position of the optical material, whose refractive index is n g , at the corresponding wavelength λ 0 , the reflectivity of the designed film system is zero, where:
[0081] n g =f(x g ), x g =(a+b) / 2;
[0082] S32. The optical material is optical glass, and is used as a substrate for film system design. The refractive index of the corresponding film layer in the film system is as follows:
[0083] Refractive index of silicon dioxide: η 1 =n SiO2 ;
[0084] Tantalum pentoxide refractive index: η 2 =n Ta2O5 ;
[0085] Substrate refractive index: η g =n glass ;
[0086] Refractive index of air: η a =n air ;
[0087] S33, corresponding wavelength λ 0 , calculate the phase thickness of the corresponding film layer under the corresponding physical thickness according to the film phase thickness formula:
[0088] Assume that the physical thickness of the first silicon dioxide film is d 1 , its phase thickness is:
[0089] Assume that the physical thickness of the second tantalum pentoxide film is d 2 , its phase thickness is:
[0090] Then the characteristic matrix of the film system is obtained as follows:
[0091] The first layer of silicon dioxide film features matrix:
[0092]
[0093] The second layer of tantalum pentoxide film characteristic matrix:
[0094]
[0095] The matrix formula of the film system and optical glass combination characteristics is as follows:
[0096]
[0097] Corresponding wavelength λ 0 , the calculation formula of the film reflectivity is as follows:
[0098]
[0099] S34, substituting the corresponding wavelength data into step S33, the physical thickness of each film layer when the reflectivity of the film system is zero can be obtained.
[0100] S4. Calculate the optical admittance distribution of the film system and air combination at different wavelengths. The calculation formula is as follows:
[0101]
[0102] Y=F / E=N-iK=f 2 (λ).
[0103] from Figure 2 It can be found that at different wavelengths, the optical admittance of the film system and air combination is different, corresponding to the center of the longitudinal position of the substrate (refractive index n g ) and wavelength λ 0 The optical admittance of the film system combined with air is equal to the refractive index n at the center of the longitudinal position of the substrate. g , the reflectivity is zero; at other positions on the substrate (refractive index n) and wavelength λ 0 Since the optical admittance of the film system and air combination remains unchanged, as the refractive index n and n g The difference gets bigger and bigger, and the reflectivity will get bigger and bigger.
[0104] When the optical admittance of the film system combined with air is close to or equal to the refractive index n of other positions of the substrate, the reflectivity is close to zero or zero. Figure 2 It can be obtained that when the same film thickness is prepared in vacuum on the substrate surface, the wavelength at which the reflectivity is close to zero or zero will be different, that is, at the distribution positions of basically different refractive indices, the wavelength will be different when the reflectivity is close to zero or zero.
[0105] It should be noted that Figure 2 The horizontal axis is the real number of equivalent admittance, and the vertical axis is the imaginary number of equivalent admittance.
[0106] S5. Calculate the size of the mask plate;
[0107] When the refractive index of the substrate and the optical admittance of the film system and air are approximately equal, the reflectivity of the film system is approximately zero, and the corresponding relationship between the wavelength and the refractive index distribution of the substrate is as follows:
[0108] n=f 1 (x)≈Y=f 2 (λ)
[0109] f 1 (x)≈f 2 (λ)
[0110] So: λ≈f 3 (x), a≤x≤b;
[0111] According to the film phase thickness formula in step S33, it can be known that when the film thickness changes in proportion to the wavelength, the reflectivity result of the film is not affected. Therefore, the preparation thickness of the film material at different positions of the refractive index on the substrate surface is changed through the mask plate, and the zero reflectivity wavelengths at different positions of the film material are overlapped, that is, the ultra-low reflection loss of the entire substrate surface after coating is obtained, which is approximately zero;
[0112] When there is no mask in front of the substrate, the refractive index n of the longitudinal center of the substrate g At wavelength λ 0 is the zero reflectivity wavelength; when a mask is installed in front of the substrate and the overall width of the mask is ω, the refractive index n at the center of the longitudinal position of the substrate g At wavelength λ′ 0 is the new zero reflectivity wavelength; then the mask width is corrected to:
[0113]
[0114] And (dc) / 10≤ω≤(dc) / 4.
[0115] In this embodiment, the dimensions of the mask plate are as follows: Figure 3 As shown, Figure 3 The horizontal axis is length and the vertical axis is width.
[0116] S6, preparing a membrane system;
[0117] Select ion beam sputtering and auxiliary methods for vacuum coating (such as Figure 4As shown), during the vacuum coating process, the mask is placed in front of the substrate to change the film thickness distribution on the substrate surface, so that the film thickness gradually changes on the surface of the substrate (as shown in FIG. Figure 6 Specifically, a U.S. Veeco dual ion beam sputtering coating machine is used for vacuum coating, and the steps include:
[0118] S61, perform substrate surface quality inspection to ensure that there is no deteriorated layer, broken points or scratches on the substrate surface;
[0119] S62, using absorbent gauze dipped in a 1:1 alcohol-ether mixture by volume ratio to clean the substrate, and using a breath method to check the cleanliness of the substrate. If the surface of the substrate is evenly covered with air after the breath, it is clean. If the surface is unevenly covered with air or there are spots, further wipe it. After cleaning, load the substrate into a dual ion beam sputtering coating machine, and install a mask plate in front of the substrate;
[0120] S63, using the process parameters described in Table 1 below to perform dual ion beam sputtering to form a film layer.
[0121] Table 1 Main process parameters of dual ion beam sputtering coating
[0122]
[0123]
[0124] In the above table, 16cm RF Ar flow indicates the argon flow rate of the 16cm RF sputtering ion source; 12cm RF Arflow indicates the argon flow rate of the 12cm RF auxiliary ion source; 12cm RF O2 flow indicates the oxygen flow rate of the 12cm RF auxiliary ion source; Neut Ar flow indicates the argon flow rate of the neutralizer; 16cm RF Beam Current indicates the beam intensity of the 16cm RF sputtering ion source; 12cm RF Beam Current indicates the beam intensity of the 12cm RF auxiliary ion source; Rate indicates the rate.
[0125] When the vacuum degree of the dual ion beam sputtering coating machine reaches 6×10 -2 Pa~9×10 -2 Pa, bake the substrate at 100℃~120℃, keep the temperature constant for 30min~40min, and continue to evacuate. When the vacuum degree is 2×10 -3 Pa~3×10 -3When the pressure is 200 Pa, the substrate is cleaned for 5 min to 10 min using a 12 cm RF ion source according to the process parameters in Table 1; after cleaning, the designed tantalum pentoxide (Ta2O5) and silicon dioxide (SiO2) film thicknesses are prepared by sputtering according to the process parameters in Table 1. After the thickness preparation is completed, the ion source of the dual ion beam sputtering coating machine is turned off and the equipment is cooled.
[0126] Baking and maintaining a constant temperature on the substrate is beneficial to improving the firmness of the film on the substrate surface. Cleaning the substrate can remove dust, water stains, oil stains and other pollutants on the substrate surface to reduce the occurrence of film defects.
[0127] S7, such as Figure 5 As shown, the spectral curve of the film system is measured, and the spectral characteristics of the entire substrate surface after coating are measured using a spectrophotometer. It is measured that the reflectivity of the entire substrate surface at the required wavelength after coating is close to zero.
[0128] It should be noted that, in this embodiment, SiO 2 and Ta 2 O 5 The purity of the alcohol-ether mixture is above 99.99%, and the alcohol-ether mixture meets the requirements of GB / T 678, including ethanol (anhydrous ethanol) and ether (meeting the requirements of GB / T 12591). In addition, the present application uses TFC optical thin film software for optical thin film analysis.
[0129] It can be seen that the present application achieves ultra-low reflection loss in the utilized spectral wavelength energy by vacuum-plating a reflective low-loss film system on the surface of a non-uniform optical material, thereby specifically solving the problem that the reflectivity of the surface of a non-uniform optical material is relatively high, and its performance affects the signal-to-noise ratio, stray light, imaging contrast, etc. of the integrated device, and cannot meet the requirements for signal transmission in high-precision and cutting-edge integrated optoelectronic devices.
[0130] Specific applications:
[0131] An optical glass with dimensions of a=20 mm, b=30 mm, c=10 mm, and d=30 mm is used as a substrate to prepare an ultra-low reflection loss film with a wavelength of 0.55 μm of the non-uniform material.
[0132] The refractive index of the substrate conforms to the following linear formula:
[0133] n=f 1 (x) = 0.02x + 1.1, 10 ≤ x ≤ 30
[0134] Then: The refractive index at the center of the longitudinal dimension of the substrate: n g =f(x g )=1.5
[0135] Two membrane materials, silicon dioxide and tantalum pentoxide, were selected for preparation.Ta2O5 =2.13, n SiO2 =1.455;
[0136] That is, the refractive index at the center of the longitudinal dimension of the substrate is 1.5, the wavelength is 0.55μm, and the reflectivity is zero.
[0137] According to the relevant calculation formula in step S33, the thickness of the tantalum pentoxide film layer is 20.98 nm, and the thickness of the silicon dioxide film layer is 123.23 nm;
[0138] The combined admittance of each wavelength of the film system and air is calculated, as shown in Table 2 below:
[0139] Table 2 Combined admittance of each wavelength of the film system and air
[0140] Wavelength nm N K wavelength N K 490 1.3 -0.2 560 1.53 0.04 500 1.33 -0.18 570 1.57 0.06 510 1.36 -0.14 580 1.61 0.08 520 1.39 -0.1 590 1.66 0.1 530 1.42 -0.05 600 1.7 0.11 540 1.46 -0.02 550 1.5 0
[0141] The calculated reflectivity is approximately zero, and the corresponding relationship between wavelength and substrate position is shown in Table 3:
[0142] Table 3 Correspondence between wavelength and substrate position
[0143] Wavelength nm N K Substrate x Wavelength nm N K Substratex 490 1.3 -0.2 10 550 1.5 0 20 500 1.33 -0.18 11.5 560 1.53 0.04 21.5 510 1.36 -0.14 13 570 1.57 0.06 23.5 520 1.39 -0.1 14.5 580 1.61 0.08 25.5 530 1.42 -0.05 16 590 1.66 0.1 28 540 1.46 -0.02 18 600 1.7 0.11 30
[0144] When there is no mask plate in front of the substrate, the film system is prepared, and the wavelength of 0.55μm at the refractive index center of 1.5 is the zero reflectivity wavelength; when the overall width of the mask plate installed in front of the substrate is ω,
[0145] ω=(dc) / 5=4mm
[0146] Prepare the film system again, at the center of the longitudinal dimension of the substrate (i.e., at a refractive index of 1.5), the wavelength of 0.53 μm is the zero reflectivity wavelength; the correction results of the mask width dimension are shown in Table 4:
[0147] Table 4 Mask plate width dimension correction results
[0148] Substratex Wavelength nm Mask plate Substratex Wavelength nm Mask plate 10 490 1mm 20 550 4mm 11.5 500 1.5mm 21.5 560 4.5mm 13 510 2mm 23.5 570 5mm 14.5 520 2.5mm 25.5 580 5.5mm 16 530 3mm 28 590 6mm 18 540 3.5mm 30 600 6.5mm
[0149] According to the above calculation results, the mask plate size matching the substrate is processed.
[0150] The specific processing process is as follows:
[0151] First, the surface quality of the substrate is inspected. There is no deteriorated layer, broken points or paths on the surface, which meets the requirements of GB / T1185-2006.
[0152] Secondly, use degreased gauze dipped in a 1:1 alcohol-ether mixture to clean the substrate, and use the breath method to check the cleanliness of the parts. If the substrate surface is evenly covered with air after breathing, it is clean. If it is unevenly covered or has spots, it should be wiped further. After cleaning, it is loaded into the American Veeco dual ion beam sputtering coating machine.
[0153] Next, the mask plate is mounted in front of the substrate.
[0154] Then, vacuum is drawn. When the vacuum degree of the dual ion beam sputtering coating machine reaches 6×10 -2 Pa~9×10 -2 Pa, bake the substrate at 100℃~120℃, keep the temperature constant for 30min~40min, and continue to evacuate. When the vacuum degree reaches 2×10 -3 Pa~3×10 -3 Pa, the substrate is cleaned for 5 min to 10 min using a 12 cm RF ion source according to the process parameters in Table 1; after cleaning, the designed tantalum pentoxide film layer (thickness 20.98 nm) and silicon dioxide film layer (thickness 123.23 nm) are sputtered according to the process parameters in Table 1. After the preparation is completed, the ion source of the dual ion beam sputtering coater is turned off and the equipment is cooled.
[0155] Finally, a spectrophotometer is used to measure the spectral characteristics of the entire substrate surface of the optical material, such as Figure 7 As shown, the reflectivity of the entire substrate surface at the required wavelength is close to zero.
[0156] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a low-loss film system for reflecting the surface of a non-uniform optical material, characterized in that: The steps include: S1. Determine the refractive index distribution formula of optical materials; S2. Select membrane materials; S3. Design the film thickness; S4. Calculate the optical admittance distribution of the film system and air combination at different wavelengths; S5. Calculate the size of the mask plate; S6, preparing a membrane system; S7. Determine the film spectrum curve.
2. The method for preparing a low-loss film system for reflecting the surface of a non-uniform optical material according to claim 1, characterized in that: In step S1, assuming that the optical material is a rectangular structure with non-uniform longitudinal distribution, the longitudinal dimension is from a to b, and the transverse dimension is from c to d, then the formula for the non-uniform longitudinal distribution of the refractive index of the optical material is as follows: n=f1(x), a≤x≤b; If the optical material is a special-shaped part, the special-shaped part is enclosed by a rectangular structure, and the size of the special-shaped part is equivalent to the size of the rectangular structure.
3. The method for preparing a low-loss film system for reflecting the surface of a non-uniform optical material according to claim 2, characterized in that: In step S2, silicon dioxide and tantalum pentoxide are selected as film materials.
4. The method for preparing a low-loss film system for reflecting the surface of a non-uniform optical material according to claim 3, characterized in that: Step S3 includes the following steps: S31, select the center of the longitudinal position of the optical material, whose refractive index is n g , at the corresponding wavelength λ0, the reflectivity of the designed film system is zero, where: n g =f(x g ),x g =(a+b) / 2; S32. The optical material is optical glass, and is used as a substrate for film system design. The refractive index of the corresponding film layer in the film system is as follows: Refractive index of silicon dioxide: η1 = n SiO2 ; Tantalum pentoxide refractive index: η2=n Ta2O5 ; Substrate refractive index: η g =n glass ; Refractive index of air: η a =n air ; S33, corresponding to the wavelength λ0, calculate the phase thickness of the corresponding film layer under the corresponding physical thickness according to the film phase thickness formula: Assuming that the physical thickness of the first silicon dioxide film layer is d1, its phase thickness is: Assuming that the physical thickness of the second tantalum pentoxide film is d2, its phase thickness is: Then the characteristic matrix of the film system is obtained as follows: The first layer of silicon dioxide film features matrix: The second layer of tantalum pentoxide film characteristic matrix: The matrix formula of the film system and optical glass combination characteristics is as follows: Corresponding to the wavelength λ0, the calculation formula of the film reflectivity is as follows: S34, substituting the corresponding wavelength data into step S33, the physical thickness of each film layer when the reflectivity of the film system is zero can be obtained.
5. The method for preparing a low-loss film system for reflecting the surface of a non-uniform optical material according to claim 4, characterized in that: In step S4, the calculation formula for the optical admittance distribution of the film system and air combination at different wavelengths is as follows: Y=F / E=N-iK=f2(λ).
6. The method for preparing a low-loss film system for reflecting the surface of a non-uniform optical material according to claim 5, characterized in that: In step S5, when the refractive index of the substrate and the optical admittance of the film system and air are approximately equal, the reflectivity of the film system is approximately zero, and the corresponding relationship between the wavelength and the refractive index distribution of the substrate is as follows: n=f1(x)≈Y=f2(λ); f1(x)≈f2tλ); have to: λ≈f3(x), a≤x≤b; According to the film phase thickness formula in step S33, it can be known that when the film thickness changes in proportion to the wavelength, the reflectivity result of the film is not affected. Therefore, the preparation thickness of the film material at different positions of the refractive index on the substrate surface is changed through the mask plate, and the zero reflectivity wavelengths at different positions of the film material are overlapped, that is, the ultra-low reflection loss of the entire substrate surface after coating is obtained, which is approximately zero; When there is no mask in front of the substrate, the refractive index n of the longitudinal center of the substrate g At this point, the wavelength λ0 is the wavelength of zero reflectivity; when a mask is installed in front of the substrate and the overall width of the mask is ω, the refractive index n at the center of the longitudinal position of the substrate is g At , the wavelength λ′0 is the new zero reflectivity wavelength; then the width dimension of the mask is corrected to: And (dc) / 10≤ω≤(dc) / 4.
7. The method for preparing a low-loss film system for reflecting the surface of a non-uniform optical material according to claim 6, characterized in that: In step S6, ion beam sputtering and auxiliary methods are selected for vacuum coating. During the vacuum coating process, a mask plate is placed in front of the substrate to change the film thickness distribution on the surface of the substrate so that the film thickness gradually changes on the surface of the substrate to prepare a film system.
8. The method for preparing a low-loss film system for reflecting the surface of a non-uniform optical material according to claim 7, characterized in that: In step S6, vacuum coating is performed using a dual ion beam sputtering coating machine, and the process includes the following steps: S61, perform substrate surface quality inspection to ensure that there is no deteriorated layer, broken points or scratches on the substrate surface; S62, using absorbent gauze dipped in a 1:1 alcohol-ether mixture by volume ratio to clean the substrate, and using a breath method to check the cleanliness of the substrate. If the surface of the substrate is evenly covered with air after the breath, it is clean. If the surface is unevenly covered with air or there are spots, further wipe it. After cleaning, load the substrate into a dual ion beam sputtering coating machine, and install a mask plate in front of the substrate; S63, vacuuming, when the vacuum degree of the dual ion beam sputtering coating machine reaches 6×10 -2 Pa~9×10 -2 When the temperature is Pa, the substrate is baked at 100℃~120℃ and kept at a constant temperature for 30min~40min to improve the firmness of the film; S64, continue to evacuate, when the vacuum degree is 2×10 -3 Pa~3×10 -3 When the pressure is 0.0457 W / m2, the argon flow rate of the 12 cm RF radio frequency auxiliary ion source is adjusted to 3 sccm, the oxygen flow rate is adjusted to 25 sccm, the argon flow rate of the neutralizer is adjusted to 5 sccm, the beam intensity is adjusted to 200 mA, and the substrate surface is cleaned for 5 min to 10 min to remove dust, water stains and oil stains on the substrate surface; S65, after cleaning, adjust the argon flow rate of the 16cm RF sputtering ion source to 18sccm, the beam intensity to 600mA, adjust the argon flow rate of the 12cm RF auxiliary ion source to 3sccm, the oxygen flow rate to 25sccm, the argon flow rate of the neutralizer to 5sccm, the beam intensity to 200mA, and deposit the first tantalum pentoxide film at a rate of 0.24nm / s to a designed thickness, and then deposit the second silicon dioxide film at a rate of 0.22nm / s to a designed thickness; S66, turn off the ion source of the dual ion beam sputtering coater and cool the equipment.
9. The method for preparing a low-loss film system for reflecting the surface of a non-uniform optical material according to claim 8, characterized in that: In step S7, the spectral characteristics of the entire substrate surface after coating are measured by a spectrophotometer, and it is measured that the reflectivity of the entire substrate surface after coating at the required wavelength is close to zero.
10. The method for preparing a low-loss film system for reflecting the surface of a non-uniform optical material according to claim 8, characterized in that: The dual ion beam sputtering coating machine adopts the American Veeco dual ion beam sputtering coating machine.