Large-size WTi target material and preparation method and application thereof
Through specific raw material mixing and stage-based program sintering and pressure control processes, the problem of quality degradation and cracking of large-sized WTi targets is solved, and the preparation of high density and high purity is achieved. It is suitable for vacuum coating sputtering, and industrial batches are realized. Production.
Patent Information
- Application Number
- CN202410981722.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
AI Technical Summary
When preparing large-size WTi targets by traditional vacuum hot pressing sintering technology, the product quality decreases, is prone to cracking, has low density and purity, making it difficult to achieve industrial mass production.
Specific raw material mixing and stage-based procedural sintering and pressure control processes are adopted, including ball milling treatment, pre-pressure treatment, step-by-step heating and pressure boosting, ensuring the ambient temperature field of the sample is stable and densified, and avoiding cracking.
With a large size with a diameter of >440mm, high density and high purity WTi targets were prepared. The product quality was controllable and suitable for vacuum coating sputtering, realizing industrial mass production.
Smart Images

Figure BDA0004956272250000081 
Figure BDA0004956272250000091 
Figure HDA0004956272260000011
Abstract
Description
Technical Field
[0001] The present invention relates to the field of metal processing, and in particular to a large-size WTi target material and a preparation method and application thereof. Background Art
[0002] WTi target material is very suitable for preparing sputtering thin film target material because of its high hardness, high density and high stability. The thin film products obtained by sputtering have the comprehensive characteristics of high failure temperature, low resistivity and high oxidation resistance.
[0003] However, the size of WTi targets prepared by traditional vacuum hot pressing sintering is generally six inches or eight inches. When the same process is used to prepare larger products (such as twelve inches), the quality of the product is seriously reduced. Not only are the density, purity and other properties affected, but more frequent cracking may even occur. Although some processes using high-precision equipment or harsh conditions can prepare high-quality, large-size WTi targets, these processes cannot be achieved in industrial mass production and are not cost-effective. Summary of the invention
[0004] Based on the defects of the prior art, the purpose of the present invention is to provide an efficient and cost-effective method for preparing large-size WTi targets. Through specific raw material mixing and special stage-programmed sintering and pressure control processes, the prepared products can still meet the requirements of high density and high purity in large sizes with a diameter of >440mm, without cracking, and the comprehensive quality of the products is high, which can be industrialized and mass-produced.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A method for preparing a large-size WTi target comprises the following steps:
[0007] (1) W powder and Ti powder are mixed and ball-milled under a protective atmosphere to obtain a mixed powder;
[0008] (2) pre-pressing the mixed powder under vacuum to obtain a rough target blank;
[0009] (3) heating the rough target blank to 600-800° C. at a rate of 8-10° C. / min in a vacuum environment, then heating it to 900-1150° C. at a rate of 5-7.5° C. / min for a second time and keeping it warm for 30-60 min, and finally heating it to 1250-1350° C. at a rate of 2-4.5° C. / min for a third time and keeping it warm for 30-60 min;
[0010] (4) After the insulation is completed, the temperature is kept constant and the pressure is increased to an ambient pressure of 20 to 25 MPa at a rate of 0.25 to 0.35 MPa / min, and then the pressure is increased to an ambient pressure of 35 to 40 MPa at a rate of 0.1 to 0.2 MPa / min for a second time and the temperature and pressure are maintained for 90 to 150 minutes, cooled, and machined to obtain the large-sized WTi target.
[0011] Traditional WTi targets are mainly prepared by sintering and hot pressing. This method has a simple process and good product quality, but it is basically only for smaller target models, such as six inches or eight inches. As the size of the target increases, the uncontrollable factors in the sintering and hot pressing process will gradually increase and become difficult to control, resulting in the traditional hot pressing sintering procedure for preparing large-sized WTi targets. Not only is it easy to crack, but the grain size may not meet the requirements, the density is low, the purity is low, and the quality is not good. Therefore, in the technical solution of the present invention, the inventor mixes W powder and Ti powder and pre-presses them, and then uses a step-by-step temperature rise method to sinter the sample. For heating, a fast rate heating method is adopted in the early stage, and a medium-to-low rate heating method is adopted in the middle and late stages with insulation steps, so that the ambient temperature field of the sample is stable and not distorted, and sufficient activation energy is obtained; then a step-by-step pressurization is also adopted. This approach is not only more suitable for process equipment, but also can ensure that the target material crystals grow fully and are densified by slow creeping, without causing uneven or even local cracking. Therefore, the product quality is still controllable even in a large size of twelve inches. If traditional spinning is still used, even if the same pressure and temperature are applied, it is difficult to ensure that the processed sample has sufficient activation energy to achieve the ideal densification.
[0012] Preferably, in the mixed powder, the mass ratio of W powder to Ti powder is (88:12) to (91:9).
[0013] Preferably, the purity of the W powder is ≥99.999%, the O content is 200-250 ppm, and the C content is 10-20 ppm; the purity of the Ti powder is ≥99.95%, the O content is 2000-2500 ppm, and the C content is 40-60 ppm.
[0014] More preferably, the particle size D of the W powder and Ti is v50 5~8μm.
[0015] Preferably, in step (1), the particle size of the grinding balls during ball milling is 10 to 20 mm, the ball-to-material ratio is 1:(2 to 3), the ball milling speed is 300 to 400 r / min, and the ball milling time is 10 to 18 h.
[0016] The ball milling process can ensure uniform mixing of the product powders without introducing additional impurities, and control the O and C contents of the obtained mixed powders at a relatively low level.
[0017] More preferably, the purity of the mixed powder is ≥99.99%, the O content is 400-500 ppm, and the C content is 20-30 ppm.
[0018] Preferably, the pre-pressing treatment in step (2) is performed in a graphite mold.
[0019] More preferably, the set pressure during the pre-pressing treatment is 6 to 10 MPa, the pressure increase rate is 0.1 to 0.3 MPa / min, and the pre-pressing treatment time is 10 to 15 min.
[0020] The pre-pressing treatment can not only ensure the shape and size of the product, but also ensure the high density and better dispersion of the powders during the subsequent hot pressing and sintering process.
[0021] Preferably, in step (3), the pressure in the vacuum environment is less than 5 Pa.
[0022] Preferably, in the step (4), the temperature of the cooled WTi target is 100-200° C., and the cooled WTi target is machined on a grinder, the single feed amount during machining is 2-10 μm, and the wire cutting rate of electric spark wire cutting is 2-5 mm / min.
[0023] The WTi target material prepared by the method of the present invention has excellent quality and can be cut and processed by conventional machine tools.
[0024] Another object of the present invention is to provide a WTi target prepared by the method for preparing the large-size WTi target.
[0025] Preferably, the WTi target is a round target;
[0026] Preferably, the radius of the WTi target is greater than 440 mm.
[0027] The WTi target prepared by the preparation method of the present invention can have high purity and density, high batch stability, low C and O impurity content, and no cracking in a twelve-inch size (i.e., within the range of radius>440mm), and is very suitable for sputtering during vacuum coating.
[0028] The beneficial effect of the present invention is that the present invention provides an efficient and cost-effective method for preparing large-size WTi targets. Through specific raw material mixing and special stage-programmed sintering and pressure control processes, the prepared products can still meet the requirements of high density and high purity at a large size of diameter > 440 mm, without cracking, and the comprehensive quality of the products is high, and industrial mass production can be realized.
[0029] Instruction Manual
[0030] Figure 1 This is a physical picture of the WTi target material obtained in Example 1 of the present invention.
[0031] Figure 2 This is a schematic diagram of a scanning electron microscope under low magnification of the WTi target obtained in Example 1 of the present invention.
[0032] Figure 3 This is a schematic diagram of a scanning electron microscope under high magnification of the WTi target obtained in Example 1 of the present invention. DETAILED DESCRIPTION
[0033] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by those of ordinary skill in the art without making creative work premise belong to the protection scope of the present invention. The experimental reagents and instruments involved in the implementation of the present invention, unless otherwise specified, are all commonly used common reagents and instruments.
[0034] Example 1
[0035] An embodiment of a large-size WTi target and a preparation method thereof according to the present invention comprises the following steps:
[0036] (1) Purity> 99.999%, O content 200ppm, C content 15ppm, particle size D v50 6μm W powder and purity>99.95%, O content 2000ppm, C content 50ppm, particle size D v50 Ti powder with a mass ratio of 6 μm and a mass ratio of 90:10 wt % are mixed, and ball milling is performed in a drum ball mill under an argon protective atmosphere to obtain a mixed powder, wherein the O content of the mixed powder is 450 ppm and the C content is 25 ppm; the ball particle size used in the drum ball mill is 10 mm, the ball-to-material ratio is 1:2, the ball milling rate is 300 r / min, and the ball milling time is 18 h;
[0037] (2) placing the mixed powder in a graphite mold and paving it flat, then evacuating it to 0 MPa, increasing the pressure to 6 MPa at a rate of 0.2 MPa / min under a vacuum environment, performing a pre-pressing treatment and maintaining the pressure for 10 minutes, and releasing the pressure to 0 MPa to obtain a rough target blank;
[0038] (3) The rough target blank was heated to 600°C at a rate of 10°C / min in a vacuum environment of 0 MPa, then heated to 1050°C at a rate of 6°C / min for a second time and kept at that temperature for 30 min, and finally heated to 1320°C at a rate of 4°C / min for a third time and kept at that temperature for 60 min;
[0039] (4) After the insulation is completed, the temperature is kept constant and the pressure is increased to 25 MPa at a rate of 0.35 MPa / min, and then the pressure is increased to 35 MPa at a rate of 0.15 MPa / min, and the temperature and pressure are maintained for 120 min. The target is cooled to 100° C. and machined on a grinder. The single feed amount during machining is 5 μm, and the wire cutting rate of the electric spark wire cutting is 3 mm / min, so as to obtain the 12-inch round WTi target. Figure 1 shown.
[0040] Example 2
[0041] An embodiment of a large-size WTi target and a preparation method thereof according to the present invention comprises the following steps:
[0042] (1) Same as step (1) of Example 1;
[0043] (2) Same as step (2) of Example 1;
[0044] (3) The rough target blank was heated to 600°C at a rate of 10°C / min in a vacuum environment of 0 MPa, then heated to 1050°C at a rate of 6°C / min for a second time and kept at that temperature for 30 min, and finally heated to 1300°C at a rate of 4°C / min for a third time and kept at that temperature for 60 min;
[0045] (4) Same as step (4) in Example 1.
[0046] Example 3
[0047] An embodiment of a large-size WTi target and a preparation method thereof according to the present invention comprises the following steps:
[0048] (1) Same as step (1) of Example 1;
[0049] (2) Same as step (2) of Example 1;
[0050] (3) The rough target blank was heated to 600°C at a rate of 10°C / min in a vacuum environment of 0 MPa, then heated to 1050°C at a rate of 6°C / min for a second time and kept at that temperature for 30 min, and finally heated to 1300°C at a rate of 4°C / min for a third time and kept at that temperature for 60 min;
[0051] (4) After the insulation is completed, the temperature is kept constant and the pressure is increased to 25 MPa at a rate of 0.35 MPa / min. Then, the pressure is increased to 30 MPa at a rate of 0.15 MPa / min and the temperature and pressure are maintained for 120 min. The target is cooled to 100° C. and machined on a grinder. The single feed amount during machining is 5 μm, and the wire cutting rate of the electric spark wire cutting is 3 mm / min, thereby obtaining the twelve-inch round WTi target.
[0052] Example 4
[0053] An embodiment of a large-size WTi target and a preparation method thereof according to the present invention comprises the following steps:
[0054] (1) Same as step (1) of Example 1;
[0055] (2) Same as step (2) of Example 1;
[0056] (3) The rough target blank was heated to 600°C at a rate of 10°C / min in a vacuum environment of 0 MPa, then heated to 1050°C at a rate of 6°C / min for a second time and kept at that temperature for 30 min, and finally heated to 1275°C at a rate of 4°C / min for a third time and kept at that temperature for 60 min;
[0057] (4) After the insulation is completed, the temperature is kept constant and the pressure is increased to 25 MPa at a rate of 0.35 MPa / min. Then, the pressure is increased to 30 MPa at a rate of 0.15 MPa / min and the temperature and pressure are maintained for 120 min. The target is cooled to 100° C. and machined on a grinder. The single feed amount during machining is 5 μm, and the wire cutting rate of the electric spark wire cutting is 3 mm / min, thereby obtaining the twelve-inch round WTi target.
[0058] Example 5
[0059] An embodiment of a large-size WTi target and a preparation method thereof according to the present invention comprises the following steps:
[0060] (1) Same as step (1) of Example 1;
[0061] (2) Same as step (2) of Example 1;
[0062] (3) The rough target blank was heated to 600°C at a rate of 10°C / min in a vacuum environment of 0 MPa, then heated to 1050°C at a rate of 6°C / min for a second time and kept at that temperature for 30 min, and finally heated to 1250°C at a rate of 4°C / min for a third time and kept at that temperature for 60 min;
[0063] (4) After the insulation is completed, the temperature is kept constant and the pressure is increased to 25 MPa at a rate of 0.35 MPa / min. Then, the pressure is increased to 30 MPa at a rate of 0.15 MPa / min and the temperature and pressure are maintained for 120 min. The target is cooled to 100° C. and machined on a grinder. The single feed amount during machining is 5 μm, and the wire cutting rate of the electric spark wire cutting is 3 mm / min, thereby obtaining the twelve-inch round WTi target.
[0064] Comparative Example 1
[0065] A large-size WTi target and a preparation method thereof, the preparation method comprising the following steps:
[0066] (1) Same as step (1) of Example 1;
[0067] (2) Same as step (2) of Example 1;
[0068] (3) heating the rough target blank to 1300°C at a rate of 10°C / min in a vacuum environment of 0 MPa and keeping the temperature for 90 min;
[0069] (4) Same as step (4) in Example 1.
[0070] Comparative Example 2
[0071] An embodiment of a large-size WTi target and a preparation method thereof, the preparation method comprising the following steps:
[0072] (1) Same as step (1) of Example 1;
[0073] (2) Same as step (2) of Example 1;
[0074] (3) Same as step (3) of Example 1;
[0075] (4) After the insulation is completed, the temperature is kept constant and the temperature is maintained at 40 MPa at a rate of 0.35 MPa / min for 120 min, cooled to 100° C., and machined on a grinder. The single feed amount during machining is 5 μm, and the wire cutting rate of the electric spark wire cutting is 3 mm / min, so as to obtain the twelve-inch round WTi target.
[0076] Comparative Example 3
[0077] An embodiment of a large-size WTi target and a preparation method thereof, the preparation method comprising the following steps:
[0078] (1) Same as step (1) of Example 1;
[0079] (2) Same as step (2) of Example 1;
[0080] (3) The rough target blank was heated to 950°C at a rate of 10°C / min in a vacuum environment of 0 MPa and kept at this temperature for 30 min, and finally heated to 1320°C at a rate of 4°C / min for a second time and kept at this temperature for 60 min;
[0081] (4) Same as step (4) in Example 1.
[0082] Comparative Example 4
[0083] An embodiment of a large-size WTi target and a preparation method thereof, the preparation method comprising the following steps:
[0084] (1) Same as step (1) of Example 1;
[0085] (2) Same as step (2) of Example 1;
[0086] (3) Same as step (3) of Example 1;
[0087] (4) After the insulation is completed, the temperature is kept constant and the pressure is increased to 35 MPa at a rate of 0.35 MPa / min to the ambient pressure and the temperature and pressure are maintained for 200 min, then cooled to 100° C. and machined on a grinder. The single feed amount during the machining is 5 μm, and the wire cutting rate of the electric spark wire cutting is 3 mm / min, thereby obtaining the twelve-inch round WTi target.
[0088] Comparative Example 5
[0089] An embodiment of a large-size WTi target and a preparation method thereof, the preparation method comprising the following steps:
[0090] (1) Same as step (1) of Example 1;
[0091] (2) Same as step (2) of Example 1;
[0092] (3) The rough target blank is heated to 600°C at a rate of 10°C / min in a vacuum environment of 0 MPa, and at the same time, the pressure is increased to an ambient pressure of 35 MPa at a rate of 0.35 MPa / min and the temperature is maintained, and then the temperature is increased to 1050°C at a rate of 6°C / min for a second time and kept at this temperature for 30 min, and finally the temperature is increased to 1320°C for a third time at a rate of 4°C / min and kept at this temperature for 150 min, cooled to 100°C, and machined on a grinder, wherein the single feed amount during the machining is 5 μm, and the wire cutting rate of the electric spark wire cutting is 3 mm / min, to obtain the twelve-inch round WTi target.
[0093] Effect Example 1
[0094] In order to verify the performance effect of the product of the present invention, the target products prepared in each embodiment and comparative example were tested for purity and Ti, O, and C element content, and then the density of the product was tested by drainage method, and the product was observed by electron microscopy to observe the grain size of W and Ti, and to observe whether it is uniform and dense, and whether there are pore defects. The test results are shown in Table 1.
[0095] Table 1
[0096]
[0097]
[0098] It can be seen from Table 1 that the WTi target material of the present invention can still achieve a high purity of more than 99.99% in a large size of 12 inches, and the density can reach more than 97%, and the highest can reach 99.8%. Figure 2 and 3 As shown, the grain size is small, dense and uniform, and there is no obvious hole defect. According to Examples 1 to 4, it can be seen that during the staged sintering and pressurizing process of the present invention, as the temperature and pressure change, the density of the product also changes to a certain extent. The main reason is that the setting of temperature and pressure affects the creep of the grains, which in turn causes a certain change in the compactness and uniformity of the stacking phase.
[0099] In contrast, although Comparative Examples 1 and 2 also adopt the process of heating first and then pressurizing, the heating program in Comparative Example 1 does not adopt a staged type, and the pressurizing program in Comparative Example 2 does not adopt a staged type. Even if the pressure is increased to more than 35MPa, the mixed powder still does not obtain enough activation energy to form a dense phase, and the product quality is poor; Comparative Example 3 is similar to the process of the embodiment, but in the heating program, the temperature zone platform range is improperly set, the degree of grain growth is insufficient, the degree of creep densification is insufficient, and the product performance is not ideal; the process described in Comparative Example 4 reduces the pressure after pressurization on the basis of Comparative Example 2 to the same as that of Example 1, and at the same time prolongs the time of heat preservation and pressure holding, but the product performance is still poor, and the Ti grain size is also large, indicating that without the implementation of staged pressurization, pressurization or prolonging the pressure holding time cannot improve the density of the product. The method described in Comparative Example 5 is a traditional preparation process system in which heating and pressurization are carried out simultaneously. The product prepared in this way has low quality at large sizes and cannot meet the use standards.
[0100] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a large-size WTi target. It is characterized in that The following steps are involved: (1) W powder and Ti powder are mixed and ball-milled under a protective atmosphere to obtain a mixed powder; (2) pre-pressing the mixed powder in a vacuum environment to obtain a rough target blank; (3) heating the rough target blank to 600-800° C. at a rate of 8-10° C. / min in a vacuum environment, then heating it to 900-1150° C. at a rate of 5-7.5° C. / min for a second time and keeping it warm for 30-60 min, and finally heating it to 1250-1350° C. at a rate of 2-4.5° C. / min for a third time and keeping it warm for 30-60 min; (4) After the insulation is completed, the temperature is kept constant and the pressure is increased to an ambient pressure of 20 to 25 MPa at a rate of 0.25 to 0.35 MPa / min, and then the pressure is increased to an ambient pressure of 35 to 40 MPa at a rate of 0.1 to 0.2 MPa / min for a second time and the temperature and pressure are maintained for 90 to 150 minutes, cooled, and machined to obtain the large-sized WTi target.
2. The method for preparing a large-size WTi target according to claim 1, It is characterized in that In the mixed powder, the mass ratio of W powder to Ti powder is (88:12) to (91:9).
3. The method for preparing the large-size WTi target according to claim 1, It is characterized in that The purity of the W powder is ≥99.999%, the O content is 200-250ppm, and the C content is 10-20ppm; the purity of the Ti powder is ≥99.95%, the O content is 2000-2500ppm, and the C content is 40-60ppm.
4. The method for preparing a large-size WTi target according to claim 1, It is characterized in that In the step (1), the particle size of the grinding balls during ball milling is 10 to 20 mm, the ball-to-material ratio is 1:(2 to 3), the ball milling speed is 300 to 400 r / min, and the ball milling time is 10 to 18 h.
5. The method for preparing a large-size WTi target according to claim 1, It is characterized in that The purity of the mixed powder is ≥99.99%, the O content is 400-500 ppm, and the C content is 20-30 ppm.
6. The method for preparing a large-size WTi target according to claim 1, It is characterized in that The set pressure during the pre-pressing treatment is 6-10 MPa, the pressure increase rate is 0.1-0.3 MPa / min, and the pre-pressing treatment time is 10-15 minutes.
7. The method for preparing a large-size WTi target according to claim 1, It is characterized in that In the step (4), the temperature of the cooled WTi target is 100-200° C., and the cooled WTi target is machined on a grinder. The single feed amount during machining is 2-10 μm, and the wire cutting rate of the electric spark wire cutting is 2-5 mm / min.
8. The WTi target material prepared by the method for preparing a large-size WTi target material according to any one of claims 1 to 7.