Graphite boat body coated with pyrolytic carbon coating as well as preparation method and application of graphite boat body
The formation of a pyrolytic carbon coating through high-temperature purification treatment and chemical vapor deposition solves the problem of reaction and coating cracks of graphite boats in working atmosphere, improves the density and high-temperature mechanical properties of graphite boats, extends the service life and reduces the Production cost.
Patent Information
- Application Number
- CN202411103150.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-08
AI Technical Summary
Graphite boats are easy to react in working atmosphere and are difficult to clean. Moreover, the thermal expansion coefficients of metal oxide coatings and graphite substrates vary greatly, resulting in poor cracks and bonding strength of the coating and short service life.
The high-temperature purification treatment and chemical vapor deposition method are used to form a pyrolytic carbon coating on the surface of the graphite boat, which enhances the density and binding force of the graphite boat, reduces the porosity and breathability, and improves the high-temperature mechanical properties of the graphite boat through the carbon density enhancement process. .
The high purity, excellent high temperature mechanical properties and service life of the graphite boat are achieved, reducing the production cost of solar cell cells, avoiding carburizing, and improving the yield rate of silicon wafers.
Smart Images

Figure CN118910585A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of graphite boats, and in particular relates to a graphite boat body covered with a pyrolytic carbon coating, and a preparation method and application thereof. Background Art
[0002] Graphite boat is a carrier used for coating in the production process of solar monocrystalline silicon and polycrystalline silicon cells. It is widely used in photovoltaic tube and slab process solar cell coating and plasma enhanced chemical vapor deposition (PE CVD) polycrystalline silicon solar cells.
[0003] However, graphite boats are prone to reaction in the working atmosphere, difficult to clean after reaction, and the material itself is prone to slag. Therefore, in order to ensure product quality and reduce problems such as boat sticking and carburization during the reaction, an isolation layer needs to be added to the surface of the graphite substrate. At present, the isolation layer on the surface of the graphite substrate generally adopts a metal oxide coating, but due to the large difference in thermal expansion coefficient between the metal oxide coating and the graphite substrate, it is easy to cause cracks in the coating, and the metal oxide coating has poor thermal shock resistance and poor bonding strength with the graphite substrate, and is prone to cracking and slag.
[0004] Therefore, the current graphite boats with metal oxide coatings on the surface are prone to failure and have a short service life. Summary of the invention
[0005] The purpose of the present invention is to provide a graphite boat covered with a pyrolytic carbon coating, and a preparation method and application thereof. The graphite boat covered with a pyrolytic carbon coating prepared by the present invention has the advantages of high purity, excellent high-temperature mechanical properties and long service life, and provides a practical and effective method for large-scale industrial production.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a graphite boat covered with a pyrolytic carbon coating, comprising the following steps:
[0008] The graphite boat body is heated to a purification treatment temperature, and the graphite boat body is purified by using a mixed purification gas to obtain a purified graphite boat body; the mixed purification gas includes a purification gas and a protective gas, and the purification gas is Freon;
[0009] Carbon densification is performed on the surface of the purified graphite boat blank to obtain a pyrolytic carbon coating, thereby obtaining the graphite boat covered with the pyrolytic carbon coating.
[0010] Preferably, the density of the graphite boat blank is greater than 1.8 g / cm 3 .
[0011] Preferably, the temperature of the purification treatment is 2000-2500°C.
[0012] Preferably, the protective gas is an inert gas, and the purity of the inert gas is ≥99.9%;
[0013] The volume ratio of the purified gas to the protective gas is (1-2):1.
[0014] Preferably, the purification process is performed cyclically;
[0015] The steps of a single purification treatment include: evacuating the purification treatment environment to the ultimate vacuum, ventilating, and performing heat preservation and pressure purification treatment after the ventilation is completed; the ventilation is to simultaneously introduce the purification gas and the protective gas; the ultimate vacuum is 2 to 10 kPa, and the flow rate of the purification gas is 1 to 20 m / s. 3 / h, the flow rate of the protective gas is 1-20m 3 / h, the ventilation time is 3 to 10 minutes, and the heat preservation and pressure purification time is 5 to 10 minutes.
[0016] Preferably, the purification process is repeated 50 to 70 times.
[0017] Preferably, the carbon densification is performed by chemical vapor deposition; the carbon densification is performed cyclically, and the number of cycles of the carbon densification is 1 to 3 times; the thickness of the pyrolytic carbon coating is 100 to 400 μm.
[0018] Preferably, the chemical vapor deposition conditions include: the carbon source gas includes methane or propylene; the flow rate of the carbon source gas is 1 to 20 m / s; 3 / h; the deposition temperature is 1000-1200°C; the deposition pressure is 2.0-10.0 kPa; the heating rate from room temperature to the deposition temperature is 40-80°C / h; and the time for each deposition is 100-300 hours.
[0019] The present invention provides a graphite boat covered with a pyrolytic carbon coating and prepared by the preparation method described in the above technical solution.
[0020] The present invention provides the use of the graphite boat covered with a pyrolytic carbon coating as described in the above technical solution in the preparation of solar cell sheets.
[0021] The present invention provides a method for preparing a graphite boat body covered with a pyrolytic carbon coating, comprising the following steps: heating a graphite boat body to a purification treatment temperature, purifying the graphite boat body with a mixed purification gas to obtain a purified graphite boat body; the mixed purification gas comprises a purification gas and a protective gas, and the purification gas is Freon; performing carbon densification on the surface of the purified graphite boat body to obtain a pyrolytic carbon coating, and obtaining the graphite boat body covered with a pyrolytic carbon coating. The preparation method provided by the present invention first improves the graphitization degree of the graphite boat body through purification treatment, enhances the high-temperature mechanical properties of the graphite boat product, and also helps to improve the bonding force between the pyrolytic carbon coating and the graphite substrate; then the present invention obtains a pyrolytic carbon coating on the surface of the graphite boat body through a carbon densification method, and the thermal expansion coefficients of the two are similar, which can effectively avoid the problems of coating cracking and slagging. Moreover, the pyrolytic carbon coating can enhance the compactness of the graphite boat, reduce the open porosity and air permeability, and further reduce the gas saturation adsorption time in the early stage of the reaction, thereby effectively reducing the production cost of solar monocrystalline silicon and polycrystalline silicon cells; at the same time, it can avoid the occurrence of carburization and improve the yield of silicon wafers. In summary, the present invention combines the high-temperature purification process and the carbon densification process to prepare a high-purity graphite boat with the advantages of high purity, excellent high-temperature mechanical properties, and long service life, providing a practical and effective method for large-scale industrial production.
[0022] Furthermore, in the present invention, the carbon densification is performed by chemical vapor deposition. The present invention adopts the chemical vapor deposition method to obtain a dense and uniform pyrolytic carbon coating, further enhancing the density of the graphite boat and reducing the open porosity and air permeability.
[0023] Furthermore, in the present invention, the carbon densification is carried out in a cycle, and the number of cycles of the carbon densification is 1 to 3 times; the thickness of the pyrolytic carbon coating is 100 to 400 μm. The present invention achieves a significant reduction in the surface open porosity of the graphite boat product under the condition of a slight increase in the product density by controlling the thickness of the pyrolytic carbon coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a schematic diagram of the structure of a conventional graphite boat blank on the market;
[0025] Figure 2 This is a partial enlarged picture of a conventional graphite boat blank on the market. DETAILED DESCRIPTION
[0026] The present invention provides a method for preparing a graphite boat covered with a pyrolytic carbon coating, comprising the following steps:
[0027] The graphite boat body is heated to a purification treatment temperature, and the graphite boat body is purified by using a mixed purification gas to obtain a purified graphite boat body; the mixed purification gas includes a purification gas and a protective gas, and the purification gas is Freon;
[0028] Carbon densification is performed on the surface of the purified graphite boat blank to obtain a pyrolytic carbon coating, thereby obtaining the graphite boat covered with the pyrolytic carbon coating.
[0029] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.
[0030] The present invention heats the graphite boat body to a purification treatment temperature, and uses a mixed purification gas to purify the graphite boat body to obtain a purified graphite boat body; the mixed purification gas includes a purification gas and a protective gas, and the purification gas is Freon. In the present invention, the graphite boat body is preferably a commercially available product. The graphite boat body is specifically a commercially available graphite boat body customized according to the drawings. The density of the graphite boat body is preferably >1.8g / cm 3 . The temperature of the purification treatment is preferably 2000-2500°C, more preferably 2100-2400°C, and specifically preferably 2300°C. The purification treatment is preferably carried out in a purification furnace. The protective gas is preferably an inert gas, and the inert gas is specifically preferably argon. The purity of the inert gas is preferably ≥99.9%, more preferably ≥99.99%. The purity of the Freon is preferably ≥99%. The volume ratio of the purified gas to the protective gas is (1-2):1, more preferably 2:1.
[0031] In the present invention, the purification treatment is preferably carried out in a cycle. The steps of a single purification treatment preferably include: evacuating the purification treatment environment to the ultimate vacuum, ventilating, and performing heat preservation and pressure purification treatment after the ventilation is completed. The ventilation is preferably to introduce purification gas and protective gas at the same time; the ultimate vacuum is preferably 2 to 10 kPa, more preferably 5 to 8 kPa. The flow rate of the purified gas is preferably 1 to 20 m 3 / h, more preferably 5 to 15m 3 / h, preferably 10m 3 The flow rate of the protective gas is preferably 1 to 20 m / h. 3 / h, more preferably 5 to 15m 3 / h, preferably 5m 3 / h. The ventilation time is preferably 3 to 10 minutes, more preferably 5 to 7 minutes, and particularly preferably 3 minutes. The heat preservation and pressure purification time is preferably 5 to 10 minutes, more preferably 5 to 7 minutes, and particularly preferably 5 minutes.
[0032] The number of cycles of the purification treatment is preferably 50 to 70 times, more preferably 55 to 65 times, particularly preferably 60 times.
[0033] In the present invention, after the purification treatment is completed, the purification furnace used in the purification treatment is preferably shut down and cooled to obtain the purified graphite boat blank.
[0034] After obtaining the graphite boat blank, the present invention performs carbon densification on the surface of the purified graphite boat blank to obtain a pyrolytic carbon coating, thereby obtaining the graphite boat covered with the pyrolytic carbon coating. In the present invention, the carbon densification is preferably performed by chemical vapor deposition. The carbon densification is preferably performed cyclically, and the number of cycles of the carbon densification is preferably 1 to 3 times, and specifically preferably 1, 2 or 3 times. The thickness of the pyrolytic carbon coating is 100 to 400 μm, more preferably 150 to 350 μm, and specifically preferably 150 μm, 250 microns or 350 μm. In the present invention, the conditions of the chemical vapor deposition preferably include: the carbon source gas preferably includes methane or propylene, and more preferably methane. The flow rate of the carbon source gas is preferably 1 to 20 m 3 / h, more preferably 5 to 15m 3 / h. The deposition temperature is preferably 1000-1200°C, more preferably 1050-1150°C. The deposition pressure is preferably 2.0-10.0 kPa, more preferably 5-8 kPa. The heating rate from room temperature to the deposition temperature is preferably 40-80°C / h, more preferably 50-70°C / h, and specifically preferably 60°C / h. The time for each deposition is preferably 100-300h, more preferably 150-250h.
[0035] The present invention provides a graphite boat covered with a pyrolytic carbon coating and prepared by the preparation method described in the above technical solution.
[0036] In the present invention, the density of the graphite boat covered with the pyrolytic carbon coating is ≥1.84 g / cm 3 , preferably 1.84 to 1.89 g / cm 3The open porosity of the graphite boat covered with the pyrolytic carbon coating is ≤1.78%, preferably 0.39-1.78%. The compressive strength of the graphite boat covered with the pyrolytic carbon coating is ≥90MPa, preferably 90.1-93.2MPa. The flexural strength of the graphite boat covered with the pyrolytic carbon coating is ≥64MPa, preferably 64.1-65.1MPa. The metal elements in the graphite boat covered with the pyrolytic carbon coating include Li, Mg, Al, Ti, Cr, Fe, Cu and Zn. The content of Li in the graphite boat covered with the pyrolytic carbon coating is less than 0.01ppm, the content of Mg is less than 0.05ppm, the content of Al is 0.08ppm, the content of Ti is less than 0.01ppm, the content of Cr is less than 0.01ppm, the content of Fe is 0.2ppm, the content of Cu is less than 0.05ppm, and the content of Zn is less than 0.05ppm.
[0037] The present invention provides the use of the graphite boat covered with a pyrolytic carbon coating as described in the above technical solution in the preparation of solar cell sheets.
[0038] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0039] Example 1
[0040] A commercially available customized high-density graphite boat was placed in a high-temperature purification furnace. After the purification furnace was heated to 2300°C and the furnace was evacuated to an ultimate vacuum of 5kPa, Freon (purity 99%) and argon (purity of argon was 99.99%) were introduced at the same time. The volume ratio of Freon to argon was 2:1, and the flow rate of Freon was 10m / s. 3 / h, the flow rate of argon is 5m 3 / h, after ventilation for 3min, ventilation was stopped, and the purification treatment was carried out by heat preservation and pressure maintenance for 5min, completing the above-mentioned first purification treatment. In this embodiment, the purification treatment was cyclically carried out, and according to the above-mentioned purification treatment process of vacuuming, ventilation and heat preservation and pressure maintenance, the purification treatment of vacuuming and ventilation was cyclically carried out 60 times, and then the furnace was stopped for cooling to obtain a purified graphite boat.
[0041] Use graphite kit to build tooling, and use CVD vapor deposition furnace to treat purified graphite boat with chemical vapor deposition pyrolytic carbon coating. The conditions of chemical vapor deposition pyrolytic carbon coating are as follows: the carbon source gas used for deposition is methane, and the methane flow rate is 10m 3 / h, the deposition heating rate is 60℃ / h, the deposition temperature is 1200℃, the deposition time is 100h, the deposition pressure is 5kPa, and the cycle is repeated once to obtain a graphite boat covered with a pyrolytic carbon coating. The thickness of the pyrolytic carbon coating is about 150μm.
[0042] Example 2
[0043] A commercially available customized high-density graphite boat was placed in a high-temperature purification furnace. After the purification furnace was heated to 2300°C and the furnace was evacuated to an ultimate vacuum of 5kPa, Freon (purity 99%) and argon (purity of argon was 99.99%) were introduced at the same time. The volume ratio of Freon to argon was 2:1, and the flow rate of Freon was 10m / s. 3 / h, the flow rate of argon is 5m 3 / h, ventilation for 3min, then stop ventilation, keep warm and keep pressure for 5min to purify, and complete the above first purification process. In this embodiment, the purification process is cyclically carried out, according to the above purification process of vacuuming, ventilation and keeping warm and keeping pressure, and the purification process is cyclically carried out 60 times in total, and then the furnace is stopped for cooling to obtain a purified graphite boat.
[0044] Use graphite kit to build tooling, and use CVD vapor deposition furnace to treat purified graphite boat with chemical vapor deposition pyrolytic carbon coating. The conditions of chemical vapor deposition pyrolytic carbon coating are as follows: the carbon source gas used for deposition is methane, and the methane flow rate is 10m 3 / h, the deposition heating rate is 60℃ / h, the deposition temperature is 1200℃, the deposition time is 100h, the deposition pressure is 5kPa, and the cycle is repeated twice to obtain a graphite boat covered with a pyrolytic carbon coating. The thickness of the pyrolytic carbon coating is about 250μm.
[0045] Example 3
[0046] A commercially available customized high-density graphite boat was placed in a high-temperature purification furnace. After the purification furnace was heated to 2300°C and the furnace was evacuated to an ultimate vacuum of 5kPa, Freon (purity 99%) and argon (purity of argon was 99.99%) were introduced simultaneously. The volume ratio of Freon to argon was 2:1, and the flow rate of Freon gas was 10m / s. 3 / h, the flow rate of argon is 5m 3 / h, ventilation for 3min, then stop ventilation, keep warm and keep pressure for 5min to purify, and complete the above first purification process. In this embodiment, the purification process is cyclically carried out, according to the purification process of vacuuming, ventilation and keeping warm and keeping pressure, and after a total of 60 cycles of purification, the furnace is stopped for cooling to obtain a purified graphite boat.
[0047] Use graphite kit to build tooling, and use CVD vapor deposition furnace to treat purified graphite boat with chemical vapor deposition pyrolytic carbon coating. The conditions of chemical vapor deposition pyrolytic carbon coating are as follows: the carbon source gas used for deposition is methane, and the methane flow rate is 10m 3 / h, the deposition heating rate is 60℃ / h, the deposition temperature is 1200℃, the deposition time is 100h, the deposition pressure is 5kPa, and the cycle is repeated 3 times to obtain a graphite boat covered with a pyrolytic carbon coating. The thickness of the pyrolytic carbon coating is about 350μm.
[0048] Test Case
[0049] (1) The density and porosity of conventional graphite boats on the market (referred to as graphite boats, without coating on the surface, Anhui Honglang Carbon Technology Co., Ltd.) and high-purity graphite boats prepared in Examples 1 to 3 were measured by drainage method. The results are shown in Table 1:
[0050] Table 1 Density and porosity test results of high purity graphite boats prepared in Examples 1 to 3
[0051] Test products <![CDATA[Density (g / cm 3 )]]> Opening rate (%) Graphite boat 1.82 15.64 Graphite boat prepared in Example 1 1.84 1.78 Graphite boat prepared in Example 2 1.87 0.54 Graphite boat prepared in Example 3 1.89 0.39
[0052] The data in Table 1 measured by the drainage method show that the high-purity graphite boats prepared in Examples 1 to 3 of the present invention have a slightly higher density than commercially available graphite boats, but a significantly lower porosity, and the porosity of the high-purity graphite boat can be further adjusted and controlled with the adjustment of process parameters. The increase in porosity can effectively reduce the saturated adsorption time of the atmosphere when the graphite boat is used, further saving time, reducing energy consumption, and saving costs.
[0053] (2) Mechanical properties test The mechanical properties of the high-purity graphite boats prepared in Examples 1 to 3 and conventional graphite boats on the market are shown in Table 2, where the compressive strength and flexural strength were tested using a three-point bending method.
[0054] Table 2 Mechanical properties of the breathable ring before and after heat treatment
[0055] project Graphite boat Example 1 Example 2 Example 3 Compressive strength / MPa 50.7 90.1 93.1 93.2 Bending strength / MPa 36.8 64.1 65.1 64.7
[0056] It can be seen from Table 2 that the mechanical properties of the high-purity graphite boat prepared by the method of the present invention are about twice that of the commercially available graphite boat, which can effectively illustrate that the high-purity graphite boat can be applied to more demanding working conditions and has a longer service life.
[0057] (3) Purity test. The purity of the high-purity graphite boat prepared in Example 3 was tested by GDMS (glow discharge mass spectrometry). The content of metal impurity elements in the purified permeable ring is shown in Table 3, unit: (ppm):
[0058] Table 3 Purity test results of high purity graphite boat prepared in Example 3
[0059] element content element content Li <0.01 Cr <0.01 Mg <0.05 Fe 0.20 Al 0.08 Cu <0.05 Ti <0.01 Zn <0.05
[0060] It can be seen from Table 3 that the high-purity graphite boat prepared in Example 3 of the present invention has the advantage of purity, can avoid the occurrence of carburization, improve the yield rate of silicon wafers, and provide a practical and effective method for large-scale industrial production.
[0061] From the above examples, it can be seen that the high-purity graphite boat prepared by the present invention in combination with the high-temperature purification process and the carbon densification process has the advantages of high purity, excellent high-temperature mechanical properties, and long service life, providing a practical and effective method for large-scale industrial production.
[0062] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing a graphite boat covered with a pyrolytic carbon coating, characterized in that: The following steps are involved: The graphite boat body is heated to a purification treatment temperature, and the graphite boat body is purified by using a mixed purification gas to obtain a purified graphite boat body; the mixed purification gas includes a purification gas and a protective gas, and the purification gas is Freon; Carbon densification is performed on the surface of the purified graphite boat blank to obtain a pyrolytic carbon coating, thereby obtaining the graphite boat covered with the pyrolytic carbon coating.
2. The preparation method according to claim 1, characterized in that: The density of the graphite boat blank is > 1.8 g / cm 3 .
3. The preparation method according to claim 1, characterized in that: The temperature of the purification treatment is 2000-2500°C.
4. The preparation method according to claim 1, characterized in that: The protective gas is an inert gas, and the purity of the inert gas is ≥99.9%; The volume ratio of the purified gas to the protective gas is (1-2):
1.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The purification process is carried out cyclically; The steps of a single purification treatment include: evacuating the purification treatment environment to the ultimate vacuum, ventilating, and performing heat preservation and pressure purification treatment after the ventilation is completed; the ventilation is to simultaneously introduce the purification gas and the protective gas; the ultimate vacuum is 2 to 10 kPa, and the flow rate of the purification gas is 1 to 20 m / s. 3 / h, the flow rate of the protective gas is 1-20m 3 / h, the ventilation time is 3 to 10 minutes, and the heat preservation and pressure purification time is 5 to 10 minutes.
6. The preparation method according to claim 5, characterized in that: The number of cycles of the purification treatment is 50 to 70 times.
7. The preparation method according to claim 1, characterized in that: The carbon densification is carried out by chemical vapor deposition; the carbon densification is carried out cyclically, and the number of cycles of the carbon densification is 1 to 3 times; the thickness of the pyrolytic carbon coating is 100 to 400 μm.
8. The preparation method according to claim 7, characterized in that: The conditions of the chemical vapor deposition include: the carbon source gas includes methane or propylene; the flow rate of the carbon source gas is 1 to 20 m 3 / h; the deposition temperature is 1000-1200°C; the deposition pressure is 2.0-10.0 kPa; the heating rate from room temperature to the deposition temperature is 40-80°C / h; and the time for each deposition is 100-300 hours.
9. A graphite boat coated with a pyrolytic carbon coating prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the graphite boat covered with pyrolytic carbon coating according to claim 9 in preparing solar cells.