Preparation method and application of Mg-MOF-74 film layer on surface of magnesium alloy micro-arc oxidation film

By growing a Mg-MOF-74 film in situ on the surface of a magnesium alloy micro-arc oxidation film, the problems of high corrosion rate and poor adhesion of MOFs in magnesium alloys have been solved, achieving efficient and environmentally friendly magnesium alloy protection and expanding its application range.

CN118910613AActive Publication Date: 2024-11-08CHONGQING UNIV +2

Patent Information

Application Number
CN202410956506.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

In existing technologies, the micro-arc oxidation film layer of magnesium alloy has micropores, resulting in a high corrosion rate. Furthermore, MOFs have poor adhesion to the magnesium alloy substrate, and the preparation method is complex, time-consuming, and not environmentally friendly.

Method used

A Mg-MOF-74 film was grown on the surface of a magnesium alloy micro-arc oxidation film by an in-situ solvothermal method. The Mg2+ in the magnesium alloy substrate and the MAO film participated in the formation of the Mg-MOF-74 film, which sealed the micropores and formed a strong bond.

Benefits of technology

The prepared Mg-MOF-74 membrane seals the pores of the MAO membrane, improving adhesion and corrosion resistance. It is suitable for applications in aerospace, automotive, and medical device fields, and is simple to operate, environmentally friendly, and energy-saving.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910613A_ABST
    Figure CN118910613A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an Mg-MOF-74 film layer on the surface of a magnesium alloy micro-arc oxidation film, which comprises the following steps: 1) immersing a magnesium alloy in a micro-arc oxidation growth solution for micro-arc oxidation treatment to obtain a magnesium alloy coated with an MAO layer; and 2) immersing the magnesium alloy coated with the MAO layer into an in-situ growth solution to carry out an in-situ solvothermal reaction, cleaning and drying to obtain the magnesium alloy coated with the Mg-MOF-74 film layer. According to the preparation method disclosed by the invention, the magnesium alloy is firstly subjected to micro-arc oxidation treatment, and then the magnesium alloy subjected to micro-arc oxidation treatment is subjected to in-situ growth reaction by adopting a traditional reaction kettle one-step in-situ solvothermal method, so that a uniform and compact Mg-MOF-74 film layer is obtained, and the corrosion resistance of the magnesium alloy is effectively improved; reagents used in the whole preparation process are simple, easy to obtain and free of environmental pollution, the whole process is simple and environmentally friendly, the requirements of industrial development and large-scale production can be met, and the application range of the magnesium alloy is widened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal surface protection treatment, and specifically relates to a preparation method and application of a Mg-MOF-74 film layer on the surface of a magnesium alloy micro-arc oxidation film. Background Art

[0002] Magnesium and its alloys are the lightest structural metals with a hexagonal crystal structure and are the eighth most abundant usable element in the Earth's crust. Magnesium alloys are used in telecommunications, batteries, torpedoes, automobiles, aerospace, biomedical and electronics industries due to their high specific strength, low weight, recyclability, low density, high damping capacity, good thermal conductivity and good castability. However, their applications are very limited due to their low standard electrode potential and high corrosion rate in water and humid environments.

[0003] Currently, there are two main solutions to solve the high corrosion rate in magnesium: the first is to alloy it with other elements by adding Mn, Zr, Al, Zn, Li, Sr and rare earth elements in different weight ratios; the second is to provide an appropriate protective film layer on its surface. The protective film layer can form an additional layer on the surface without changing the inherent properties of the alloy itself.

[0004] Micro-arc oxidation film (MAO) is the most common surface treatment method for magnesium alloys, with simple preparation technology and reliable methods. However, during the discharge breakdown process of micro-arc oxidation, the surface of the film layer contacts the electrolyte, the melt will quickly solidify and release gas, forming micropores. These micropores inherent in the surface of the MAO film layer are connecting channels for the corrosive medium to invade the substrate, causing the MAO film layer to degrade over time, thereby significantly reducing the fatigue life of the magnesium alloy. Therefore, the MAO film layer needs to be subsequently treated.

[0005] Metal-organic frameworks (MOFs) are a new type of material. They are porous network structures formed by the self-assembly of inorganic metal ions and organic ligands (heterocyclic compounds containing heteroatoms such as N and O); they are famous for their extremely high specific surface area, excellent thermal stability and chemical stability. However, MOFs have satisfactory performance in the field of corrosion protection, mainly because MOFs particles are integrated into the polymer matrix as nanofillers. This method is easily limited by the compatibility of MOFs crystals, resulting in poor dispersion stability of MOFs during the coating preparation process. Experiments have shown that MOFs cannot grow directly into films on magnesium alloy substrates due to their poor adhesion. Therefore, it is necessary to pre-treat the magnesium alloy AZ31 before growing the MOFs film layer.

[0006] In the prior art, the solvothermal method for preparing Mg-MOF-74 can only obtain MOFs powder. For example, patent CN 118165284A discloses a method for synthesizing Mg-MOF-74, which dissolves soluble magnesium salt and organic ligand in a mixed solvent composed of different proportions of N,N-dimethylformamide and a first low-carbon alcohol to obtain a mixed solution 1; then water and the mixed solution 1 are mixed in different proportions and subjected to a solvothermal reaction. The sample (crude product) after the reaction is completed needs to be separated from the solid and liquid, washed, soaked in the second low-carbon alcohol for 48-96 hours, and vacuum dried at high temperature (200-300°C) for 2-8 hours to obtain the final Mg-MOF-74 powder product with different morphologies. The method has complicated steps, requires vacuum equipment, and is time-consuming; Patent CN 115216025 A discloses a method for preparing defective Mg-MOF-74 by hydrothermal reaction, wherein MgCl2·6H2O and 2,5-dihydroxyterephthalic acid are dissolved in a mixed solvent of N,N-dimethylformamide, anhydrous ethanol, and deionized water, and then heated and allowed to stand to obtain a precipitate (crude product), and then fully stirred with a fresh methanol solution and allowed to stand for 12 hours, filtered and re-added with fresh methanol solution, repeated 6 times (3 days), and washed and dried to obtain the final Mg-MOF-74 powder crystals. The methanol solution used in this method is toxic, potentially harmful to the human body, and is time-consuming and cumbersome to operate, which is not conducive to the promotion and application of Mg-MOF-74. Summary of the invention

[0007] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the main purpose of the present invention is to provide a method for preparing a Mg-MOF-74 film layer on the surface of a magnesium alloy micro-arc oxidation film, aiming to solve the problems that the existing MOFs are not widely used in magnesium alloy corrosion protection, the raw materials are varied, the consumption is large, and the safety, environmental protection and energy-saving performance are poor.

[0008] The objective of the present invention is achieved through the following technical solutions:

[0009] A method for preparing a Mg-MOF-74 film layer on the surface of a magnesium alloy micro-arc oxidation film comprises the following steps:

[0010] 1) immersing the magnesium alloy in a micro-arc oxidation growth solution for micro-arc oxidation treatment to obtain a magnesium alloy covered with a MAO layer;

[0011] 2) The magnesium alloy coated with the MAO layer is immersed in an in-situ growth solution for an in-situ solvothermal reaction, and then cleaned and dried to obtain a magnesium alloy coated with a Mg-MOF-74 film layer, i.e., a Mg-MOF-74 film layer on the surface of the magnesium alloy MAO film.

[0012] In certain specific embodiments, the micro-arc oxidation growth solution includes an aqueous solution of 0.03-0.06 M trisodium phosphate dodecahydrate and 0.1-0.3 M sodium hydroxide.

[0013] In some specific embodiments, the process parameters of the micro-arc oxidation treatment are: the temperature of the micro-arc oxidation growth liquid is 5-10° C., the reaction voltage is 300-400 V, and the reaction time is 2-8 min.

[0014] In some specific embodiments, the in-situ growth solution includes a mixed solution of 0.2-0.4 mM magnesium nitrate and 0.3-0.5 mM trimesic acid; the mixed solution is a mixture of N-,N-dimethylformamide, anhydrous ethanol and deionized water in a volume ratio of 15:1:1.

[0015] In certain specific embodiments, the process parameters of the in-situ solvothermal reaction are: reaction temperature of 100-140° C., and reaction time of 16-32 h.

[0016] In some specific embodiments, the method further includes pre-treating the magnesium alloy before micro-arc oxidation treatment, specifically, grinding the magnesium alloy substrate first, and then degreasing and deoiling the ground magnesium alloy substrate.

[0017] In some specific embodiments, the polishing treatment is specifically: polishing the magnesium alloy substrate using 150, 600, 800, 1200, and 2000# sandpaper respectively, and ultrasonically cleaning with alcohol and then drying.

[0018] In certain specific embodiments, the degreasing and deoiling solution used in the degreasing and deoiling process is an aqueous solution including 40 g / L of sodium hydroxide, 25 g / L of sodium carbonate, and 40 g / L of sodium phosphate, based on mass volume concentration.

[0019] The purpose of the present invention is to also provide the application of the Mg-MOF-74 film layer on the surface of the aforementioned magnesium alloy micro-arc oxidation film in the fields of aerospace, automobiles, medical equipment and 3C digital.

[0020] Compared with the prior art, the present invention has at least the following advantages:

[0021] 1) The method for preparing the Mg-MOF-74 film layer on the surface of the micro-arc oxidation film of the magnesium alloy provided in the present application adopts a micro-arc oxidation growth solution of specific components, the components of which are simple and easy to obtain, which greatly shortens the time of micro-arc oxidation treatment to only 2-8 minutes, thereby greatly improving the production efficiency; at the same time, when preparing the Mg-MOF-74 film layer, a mixed solution of N-, N-dimethylformamide: anhydrous ethanol: deionized water = 15:1:1 is used as the medium, and no additional metal cations are introduced, making the production safer, more environmentally friendly and energy-saving;

[0022] 2) The method for preparing the Mg-MOF-74 film layer on the surface of the micro-arc oxidation film of the magnesium alloy provided by the present invention is to first perform micro-arc oxidation treatment on the magnesium alloy, and then use the traditional one-step in-situ solvent thermal method in a reactor to perform in-situ growth reaction on the magnesium alloy after the micro-arc oxidation treatment to obtain a uniform and dense Mg-MOF-74 film layer; the reagents used in the entire preparation process are simple, easy to obtain, and pollution-free to the environment. The overall process is simple and green and environmentally friendly, which can meet the needs of industrial development and mass production, and can further expand the application range of magnesium alloys. In addition, the traditional one-step solvent thermal method is used on the surface of the magnesium alloy MAO film layer, and the reaction conditions are mild and the process is stable; the metal cations in the magnesium alloy and MAO will participate in the formation of the Mg-MOF-74 film layer during the solvent thermal process, making the preparation method of the present invention more mature, more energy-saving, more practical for industrial production, simple to operate, etc., providing a new technical route for industrial production;

[0023] 3) The Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film prepared by the present invention is in-situ grown, and the prepared film layer is firmly bonded. The Mg-MOF-74 film layer grown on the micro-arc oxidation film layer as the substrate has good bonding force and film-forming properties, and closes the pores of the MAO film; no additional metal cations are introduced, and the magnesium alloy matrix and the Mg in the MAO film layer are bonded together. 2+ They jointly participate in the formation of the Mg-MOF-74 film layer, effectively blocking and preventing external corrosive ions (such as Cl-, etc.) from corroding the magnesium matrix, and playing a role in protecting the matrix; it is suitable for promotion and application in aerospace, automobile, medical equipment, 3C digital and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the specific embodiments of the present invention, the drawings required for use in the specific embodiments or the description of the prior art will be briefly introduced below.

[0025] Figure 1 is a scanning electron microscope photograph of the Mg-MOF-74 film layer on the surface of the magnesium alloy in Example 1;

[0026] Figure 2 is a metallographic micrograph of the Mg-MOF-74 film bonding strength test on the magnesium alloy surface in Example 1;

[0027] Figure 3 is the XRD spectrum of the Mg-MOF-74 film layer on the surface of the magnesium alloy in Example 1;

[0028] Figure 4AZ31 magnesium alloy, AZ31 magnesium alloy coated with MAO film and AZ31 magnesium alloy coated with Mg-MOF-74 film are Tafel polarization curves at the same coordinates measured by an electrochemical workstation in Example 1;

[0029] Figure 5 is a scanning electron microscope photograph of the Mg-MOF-74 film layer on the surface of the magnesium alloy in Example 2;

[0030] Figure 6 is the Tafel polarization curve of the AZ31 magnesium alloy, the AZ31 magnesium alloy coated with MAO film and the AZ31 magnesium alloy coated with Mg-MOF-74 film at the same coordinates measured by the electrochemical workstation in Example 2;

[0031] Figure 7 is a scanning electron microscope photograph of the Mg-MOF-74 film layer on the surface of the magnesium alloy in Example 3;

[0032] Figure 8 These are the Tafel polarization curves of the AZ31 magnesium alloy, the AZ31 magnesium alloy coated with MAO film, and the AZ31 magnesium alloy coated with Mg-MOF-74 film at the same coordinates measured by the electrochemical workstation in Example 3. DETAILED DESCRIPTION

[0033] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. The following embodiments are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.

[0034] When a certain amount, concentration or other value or parameter is expressed in the form of a range, a preferred range, or a preferred upper and lower numerical limit, it should be understood that it is equivalent to specifically revealing any range by combining any pair of upper range limits or preferred numerical values ​​with any lower range limit or preferred numerical value, regardless of whether the range is specifically disclosed. Unless otherwise indicated, the numerical range values ​​listed herein include the endpoints of the range, and all integers and fractions within the range.

[0035] Unless otherwise indicated, all percentages, parts, ratios, etc. herein are by weight.

[0036] The materials, methods, and examples herein are illustrative and are not to be construed as limiting unless specifically stated.

[0037] In the following examples, magnesium nitrate, trimesic acid, N-,N-dimethylformamide, anhydrous ethanol, and deionized water were purchased from Shanghai Sinopharm Chemical Reagent Co., Ltd., China;

[0038] The test methods used in the following embodiments include:

[0039] The corrosion resistance and bonding strength are reflected by testing the Tafel polarization curve of each test sample and metallographic microscopic observation of the scratch.

[0040] 1) Binding strength test;

[0041] A metallographic microscope (Zeiss, Germany) was used to form a criss-cross pattern on the surface of different coatings using a QFH-type cutter. The cut reached the Mg substrate, and then its surface was carefully cleaned five times with a brush, and tape was stuck on the cut to pull it apart. The adhesion between the coating and the AZ31 substrate was evaluated according to GB / T 9286-1998.

[0042] Example 1

[0043] The method for preparing the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film provided in this embodiment comprises the following steps:

[0044] 1) Degreasing and oil removal

[0045] 11) preparing an aqueous solution containing 40 g / L of sodium hydroxide, 25 g / L of sodium carbonate, and 40 g / L of sodium phosphate;

[0046] 12) Magnesium alloy pretreatment: Use 150#, 600#, 800#, 1200#, and 2000# sandpaper to grind the magnesium alloy, and use alcohol to ultrasonically clean it for five minutes and then dry it for use;

[0047] 13) Soak the polished magnesium alloy AZ31 in the above degreasing and deoiling aqueous solution, keep it in a water bath at 50°C for 60 seconds, then wash it with a 1M sodium hydroxide aqueous solution for 30 seconds, and then polish it with 400g / L nitric acid (ρ=1.42g / ml) at room temperature 25°C for 2 minutes; then wash it once with deionized water and blow it dry with cold air;

[0048] 2) Micro-arc oxidation film (MAO for short)

[0049] 21) Prepare a micro-arc oxidation growth solution containing 0.049 M trisodium phosphate dodecahydrate and 0.18 M sodium hydroxide using deionized water according to the molar concentration;

[0050] 22) First, the magnesium alloy sample after degreasing and deoiling in step 1) is fixed in a polymethyl methacrylate electrolytic cell equipped with a stainless steel plate by copper wire, and then the micro-arc oxidation growth solution in step 21) is poured; the anode is AZ31 magnesium alloy, and the cathode is a stainless steel plate; the temperature of the micro-arc oxidation growth solution is 8°C, the reaction voltage is 350V, and the reaction time is 5min, to obtain a magnesium alloy covered with a MAO film;

[0051] 3) In situ growth of Mg-MOF-74 film (Mg-MOF-74 for short)

[0052] 31) preparing a mixed solution of N-, N-dimethylformamide: anhydrous ethanol: deionized water = 15:1:1 (volume ratio); and dissolving magnesium nitrate and trimesic acid in the mixed solution according to the molar concentration, and mixing them evenly to obtain an in-situ growth solution; wherein the molar concentration of magnesium nitrate is 0.2 mM, and the molar concentration of trimesic acid is 0.4 mM;

[0053] 32) placing the magnesium alloy coated with the MAO film prepared in step 2) into a polytetrafluoroethylene liner sleeve, then pouring the in-situ growth solution prepared in step 31) into the liner and placing the liner into the reactor, tightening it, and finally placing it in a drying oven for in-situ growth at a reaction temperature of 120° C. for a reaction time of 24 h, washing and drying to obtain a magnesium alloy coated with a Mg-MOF-74 film;

[0054] The cleaning and drying are as follows: specifically, the magnesium alloy sample covered with the Mg-MOF-74 film layer after the reaction in step 3) is first cleaned with flowing deionized water to remove the in-situ growth liquid attached to the surface, and then the sample is ultrasonically cleaned in anhydrous ethanol for 7 minutes using an ultrasonic cleaning machine, and then cleaned with deionized water and dried to obtain the Mg-MOF-74 film layer (Mg-MOF-74 film layer) on the surface of the magnesium alloy micro-arc oxidation film.

[0055] The present application tests the morphology, structure and performance of the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film prepared in this embodiment, specifically:

[0056] 1) Appearance

[0057] The present application conducted an appearance morphology test on the Mg-MOF-74 film on the surface of the magnesium alloy in Example 1, and the electron microscope scanning image thereof is shown in FIG. Figure 1 As shown in the figure, the surface of the Mg-MOF-74 film on the magnesium alloy has completely covered the MAO film layer. The Mg-MOF-74 nanoparticles grow horizontally in a rod-like shape and are tightly connected to each other. There are also some impurities, which may be due to the Mg dissolved in the magnesium matrix and the MAO film layer. 2+ Ion related.

[0058] In addition, the metallographic micrograph of the Mg-MOF-74 film on the surface of the magnesium alloy micro-arc oxidation film is shown in Figure 2 As shown in the figure, it can be seen that the Mg-MOF-74 film layer on the surface of the micro-arc oxidation film of the magnesium alloy has a clear and smooth cutting edge, no obvious large-scale detachment is observed, and the tiny detachment area in the cross-region does not exceed 5%. According to the classification standard of bonding strength, the bonding strength between the Mg-MOF-74 film layer on the surface of the micro-arc oxidation film and the magnesium alloy is evaluated as level 1.

[0059] 2) Structural analysis

[0060] The present application tests the crystallinity of the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film in Example 1, and its XRD spectrum is as follows: Figure 3 As shown in the figure, it can be seen that the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film has multiple characteristic diffraction peaks at 7.6°, 9.2°, 27.9°, 28.5° and 29.5°. Most of these peaks are sharp and have high intensity, indicating that the Mg-MOF-74 film layer has good crystallinity.

[0061] 3) Electrochemical performance

[0062] The present application tests the electrochemical properties of the magnesium alloy surface film layer in Example 1 by using an electrochemical workstation, specifically:

[0063] The Tafel polarization curves of magnesium alloy AZ31, magnesium alloy coated with MAO film (curve MAO) and magnesium alloy coated with Mg-MOF-74 film (curve Mg-MOF-74) measured by electrochemical workstation at the same coordinates are as follows: Figure 4 Specifically:

[0064] The corrosion resistance test of the magnesium alloy protective film is represented by the electrochemical polarization curve (equipment model is Princeton4000A), in which the corrosion voltage of AZ31 magnesium alloy is -1.37V, the corrosion voltage of AZ31 magnesium alloy covered with MAO film after treatment under the conditions of Example 1 is -1.55V, and the corrosion voltage of AZ31 magnesium alloy covered with Mg-MOF-74 film is -1.51V. Compared with the magnesium alloy substrate, the corrosion voltage is significantly improved, the corrosion tendency is reduced, and the corrosion rate and corrosion resistance are directly related to the corrosion current density. The corrosion current density of pure AZ31 magnesium alloy is 1.02×10 -5 Acm -2 The corrosion current density of the magnesium alloy covered with MAO film is 7.31×10 -7 A cm -2 However, the corrosion current density of the magnesium alloy coated with Mg-MOF-74 film after treatment under the conditions of Example 1 is 1.21×10 -7 A cm -2 The corrosion current density of the treated magnesium alloy is reduced by half an order of magnitude compared with the magnesium alloy coated with MAO film; the corrosion current density is reduced by two orders of magnitude compared with the sample of AZ31 magnesium alloy. The above results can fully illustrate that the Mg-MOF-74 film has an effective corrosion inhibition effect on AZ31 magnesium alloy, and the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film of the present invention has excellent corrosion resistance and can effectively protect the magnesium substrate.

[0065] Example 2

[0066] The method for preparing the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film provided in this embodiment comprises the following steps:

[0067] 1) Degreasing and oil removal

[0068] 11) preparing an aqueous solution containing 40 g / L of sodium hydroxide, 25 g / L of sodium carbonate, and 40 g / L of sodium phosphate;

[0069] 12) Pretreatment of magnesium alloy: using 150#, 600#, 800#, 1200#, and 2000# sandpaper to grind the magnesium alloy, and using alcohol to ultrasonically clean it for five minutes and then dry it for use;

[0070] 13) The polished magnesium alloy AZ31 was immersed in the above-mentioned degreasing and deoiling aqueous solution, kept in a water bath at 50°C for 60 seconds, then alkaline washed with a 1M sodium hydroxide aqueous solution for 30 seconds, and then polished with 400g / L nitric acid (ρ=1.42g / ml) at room temperature 25°C for 2 minutes; then rinsed once with deionized water and blown dry with cold air.

[0071] 2) Micro-arc oxidation film (MAO for short)

[0072] 21) Prepare a micro-arc oxidation growth solution containing 0.049 M trisodium phosphate dodecahydrate and 0.18 M sodium hydroxide using deionized water according to the molar concentration;

[0073] 22) First, the magnesium alloy sample after degreasing and deoiling in step 1) is fixed in a polymethyl methacrylate electrolytic cell equipped with a stainless steel plate by copper wire, and then the micro-arc oxidation growth solution in step 21) is poured; the anode is AZ31 magnesium alloy, and the cathode is a stainless steel plate; the temperature of the micro-arc oxidation growth solution is 8°C, the reaction voltage is 350V, and the reaction time is 5min, to obtain a magnesium alloy covered with a MAO film;

[0074] 3) In situ growth of Mg-MOF-74 film (Mg-MOF-74 for short)

[0075] 31) Using a mixed solution of N-, N-dimethylformamide: anhydrous ethanol: deionized water = 15:1:1 (volume ratio), an in situ growth solution containing 0.3 mM magnesium nitrate and 0.3 mM trimesic acid was prepared according to the molar concentration;

[0076] 32) placing the magnesium alloy with the surface MAO layer prepared in step 2) into a polytetrafluoroethylene liner sleeve, then pouring the in-situ growth solution prepared in step 31) into the liner and placing the liner into a reactor, tightening it, and finally placing it in a drying oven for in-situ growth at a reaction temperature of 110° C. for 18 h to obtain a magnesium alloy covered with a Mg-MOF-74 film;

[0077] The cleaning and drying are as follows: the magnesium alloy sample covered with the Mg-MOF-74 film layer after the reaction in step 3) is first cleaned with flowing deionized water to remove the in-situ growth liquid attached to the surface, and then the sample is ultrasonically cleaned in anhydrous ethanol for 6 minutes using an ultrasonic cleaning machine, and then cleaned with deionized water and dried to obtain the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film.

[0078] The present application tests the morphology and performance of the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film prepared in this embodiment, specifically:

[0079] 1) Appearance

[0080] The present application conducted an appearance morphology test on the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film in Example 2. The electron microscope scanning image is as follows: Figure 5 As shown in the figure, it can be seen that the surface of the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film is still completely covered with the MAO film layer, and the rod-shaped Mg-MOF-74 grows in multiple directions, with a small part growing perpendicular to the alloy matrix.

[0081] 2) Electrochemical performance

[0082] The present application tests the electrochemical properties of the magnesium alloy surface film layer in Example 2 by using an electrochemical workstation, specifically:

[0083] The Tafel polarization curves of magnesium alloy AZ31, magnesium alloy coated with MAO film (curve MAO) and magnesium alloy coated with Mg-MOF-74 film (curve Mg-MOF-74) measured by electrochemical workstation at the same coordinates are as follows: Figure 6 As shown, specifically:

[0084] The corrosion resistance test of the magnesium alloy protective film is represented by the electrochemical polarization curve (equipment model is Princeton4000A), in which the corrosion voltage of AZ31 magnesium alloy is -1.37V, the corrosion voltage of AZ31 magnesium alloy covered with MAO film after treatment under the conditions of Example 2 is -1.55V, and the corrosion voltage of AZ31 magnesium alloy covered with Mg-MOF-74 film is -1.49V. Compared with the magnesium alloy substrate, the corrosion voltage is significantly improved, the corrosion tendency is reduced, and the corrosion rate and corrosion resistance are directly related to the corrosion current density. The corrosion current density of pure AZ31 magnesium alloy is 1.02×10 -5 Acm -2 The corrosion current density of the magnesium alloy covered with MAO film is 7.31×10 -7 A cm -2However, the corrosion current density of the magnesium alloy coated with Mg-MOF-74 film after treatment under the conditions of Example 2 is 2.19×10 -7 A cm -2 The corrosion current density of the treated magnesium alloy is reduced by half an order of magnitude compared with the magnesium alloy coated with MAO film; the corrosion current density is reduced by two orders of magnitude compared with the sample of AZ31 magnesium alloy. The above results can fully illustrate that the Mg-MOF-74 film has an effective corrosion inhibition effect on AZ31 magnesium alloy, and the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film of the present invention has excellent corrosion resistance and can effectively protect the magnesium substrate.

[0085] Example 3

[0086] The method for preparing the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film provided in this embodiment comprises the following steps:

[0087] 1) Degreasing and oil removal

[0088] 11) preparing an aqueous solution containing 40 g / L of sodium hydroxide, 25 g / L of sodium carbonate, and 40 g / L of sodium phosphate;

[0089] 12) Pretreatment of magnesium alloy: using 150#, 600#, 800#, 1200#, and 2000# sandpaper to grind the magnesium alloy, and using alcohol to ultrasonically clean it for five minutes and then dry it for use;

[0090] 13) The polished magnesium alloy AZ31 was immersed in the above-mentioned degreasing and deoiling aqueous solution, kept in a water bath at 50°C for 60 seconds, then alkaline washed with a 1M sodium hydroxide aqueous solution for 30 seconds, and then polished with 400g / L nitric acid (ρ=1.42g / ml) at room temperature 25°C for 2 minutes; then rinsed once with deionized water and blown dry with cold air.

[0091] 2) Micro-arc oxidation film (MAO for short)

[0092] 21) Prepare a micro-arc oxidation growth solution containing 0.049 M trisodium phosphate dodecahydrate and 0.18 M sodium hydroxide using deionized water according to the molar concentration;

[0093] 22) First, the magnesium alloy sample after degreasing and deoiling in step 1) is fixed in a polymethyl methacrylate electrolytic cell equipped with a stainless steel plate by copper wire, and then the micro-arc oxidation growth solution in step 21) is poured; the anode is AZ31 magnesium alloy, and the cathode is a stainless steel plate; the temperature of the micro-arc oxidation growth solution is 8°C, the reaction voltage is 350V, and the reaction time is 5min, to obtain a MAO layer on the surface of the magnesium alloy;

[0094] 3) In situ growth of Mg-MOF-74 film (Mg-MOF-74 for short)

[0095] 31) Using a mixed solution of N-, N-dimethylformamide: anhydrous ethanol: deionized water = 15:1:1 (volume ratio), an in situ growth solution containing 0.4 mM magnesium nitrate and 0.5 mM trimesic acid was prepared according to the molar concentration;

[0096] 32) placing the magnesium alloy with the surface MAO layer prepared in step 2) into a polytetrafluoroethylene liner sleeve, then pouring the in-situ growth solution prepared in step 31) into the liner and placing it into a reactor, tightening it, and finally placing it in a drying oven for in-situ growth, with a reaction temperature of 140° C. and a reaction time of 30 h, to obtain a Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film, i.e., a Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film;

[0097] The cleaning and drying are as follows: the magnesium alloy sample covered with the Mg-MOF-74 film layer after the reaction in step 3) is first cleaned with flowing deionized water to remove the in-situ growth liquid attached to the surface, and then the sample is ultrasonically cleaned in anhydrous ethanol for 8 minutes using an ultrasonic cleaning machine, and then cleaned with deionized water and dried to obtain the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film.

[0098] The present application tests the morphology and performance of the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film prepared in this embodiment, specifically:

[0099] 1) Appearance

[0100] The present application conducted an appearance morphology test on the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film in Example 3. The electron microscope scanning image is as follows: Figure 7 As shown in the figure, it can be seen that the Mg-MOF-74 film on the surface of the magnesium alloy micro-arc oxidation film grows basically vertically to the substrate surface, which may be related to the 2+ Concentration related.

[0101] 2) Electrochemical performance

[0102] The present application tests the electrochemical properties of the magnesium alloy surface film layer in Example 3 by using an electrochemical workstation, specifically:

[0103] The Tafel polarization curves of magnesium alloy AZ31, magnesium alloy coated with MAO film (curve MAO) and magnesium alloy coated with Mg-MOF-74 film (curve Mg-MOF-74) measured by electrochemical workstation at the same coordinates are as follows: Figure 8 As shown, specifically:

[0104] The corrosion resistance test of the magnesium alloy protective film is represented by the electrochemical polarization curve (equipment model is Princeton4000A), in which the corrosion voltage of AZ31 magnesium alloy is -1.37V, the corrosion voltage of AZ31 magnesium alloy covered with MAO film after treatment under the conditions of Example 1 is -1.55V, and the corrosion voltage of AZ31 magnesium alloy covered with Mg-MOF-74 film is -1.42V. Compared with the magnesium alloy substrate, the corrosion voltage is significantly improved, the corrosion tendency is reduced, and the corrosion rate and corrosion resistance are directly related to the corrosion current density. The corrosion current density of pure AZ31 magnesium alloy is 1.02×10 -5 Acm -2 The corrosion current density of the magnesium alloy covered with MAO film is 7.31×10 -7 A cm -2 However, the corrosion current density of the sample coated with Mg-MOF-74 film after treatment under the conditions of Example 3 is 2.78×10 -7 A cm -2 The corrosion current density of the treated samples was reduced by half an order of magnitude compared with the magnesium alloy coated with MAO film; the corrosion current density was reduced by two orders of magnitude compared with the sample of AZ31 magnesium alloy. The above results can fully illustrate that the Mg-MOF-74 film has an effective corrosion inhibition effect on AZ31 magnesium alloy, and the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film of the present invention has excellent corrosion resistance and can effectively protect the magnesium substrate.

[0105] Comparative Example 1

[0106] The method for preparing the Mg-MOF-74 film layer on the surface of the micro-arc oxidation film of the magnesium alloy provided in this comparative example is basically the same as that of Example 2, except that the magnesium alloy is not subjected to micro-arc oxidation treatment, and the Mg-MOF-74 film is directly grown in situ on the magnesium alloy, and specifically comprises the following steps:

[0107] 1) Degreasing and oil removal

[0108] 11) preparing an aqueous solution containing 40 g / L of sodium hydroxide, 25 g / L of sodium carbonate, and 40 g / L of sodium phosphate;

[0109] 12) Pretreatment of magnesium alloy: using 150#, 600#, 800#, 1200#, and 2000# sandpaper to grind the magnesium alloy, and using alcohol to ultrasonically clean it for five minutes and then dry it for use;

[0110] 13) The polished magnesium alloy AZ31 was immersed in the above-mentioned degreasing and deoiling aqueous solution, kept in a water bath at 50°C for 60 seconds, then alkaline washed with a 1M sodium hydroxide aqueous solution for 30 seconds, and then polished with 400g / L nitric acid (ρ=1.42g / ml) at room temperature 25°C for 1-2min; then rinsed once with deionized water and blown dry with cold air.

[0111] 2) In situ growth of Mg-MOF-74 film (Mg-MOF-74 for short)

[0112] 21) Using a mixed solution of N-, N-dimethylformamide: anhydrous ethanol: deionized water = 15:1:1 (volume ratio), an in situ growth solution containing 0.3 mM magnesium nitrate and 0.3 mM trimesic acid was prepared according to the molar concentration;

[0113] 22) The magnesium alloy pretreated in step 1) is placed in a polytetrafluoroethylene inner liner sleeve, and then the in-situ growth liquid prepared in step 21) is poured in and the inner liner is placed in a reactor, tightened, and finally placed in a drying oven for in-situ growth. The reaction temperature is 110°C and the reaction time is 20 hours. As a result, the Mg-MOF-74 nanoparticles are dispersed and arranged in clusters on the surface of the magnesium alloy, and a magnesium alloy covered with a continuous film of Mg-MOF-74 cannot be obtained.

[0114] By comparing Example 2 with Comparative Example 1, it can be seen that in the method for preparing the Mg-MOF-74 film layer on the surface of the micro-arc oxidation film of the magnesium alloy provided in the present application, the magnesium alloy is first subjected to MAO film treatment, which is a prerequisite for realizing the solvothermal method for preparing the Mg-MOF-74 film layer, that is, the micro-arc oxidation treatment and the in-situ solvothermal reaction are synergistic, and the preparation of the Mg-MOF-74 film layer is successfully realized, and the Mg-MOF-74 film layer has excellent bonding with the magnesium alloy AZ31.

[0115] In summary, the preparation method of the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc film provided by the present invention is based on the magnesium alloy MAO film, a layer of Mg-MOF-74 film layer is in situ grown by a solvent thermal method, and the micropores of MAO are filled with Mg-MOF-74 nanoparticles, so that the film layer is denser and the corrosion resistance is better; and no additional metal cations need to be introduced, and the Mg in the magnesium alloy matrix and the MAO film layer is fully utilized. 2+; In addition, due to the in-situ growth, Mg-MOF-74 can be directly formed on the surface of the magnesium alloy MAO film, which improves the bonding strength and film-forming performance between the film layer and the substrate, and improves the feasibility of application in the industrial field. The Mg-MOF-74 film layer not only seals the pores of the MAO film layer, but also has the characteristics of corrosion resistance, and its performance is far superior to that of the untreated magnesium alloy AZ31. After a large number of experiments, the inventors found that by using a traditional and mature reactor on the MAO film layer, the purpose can be achieved through solvent thermal reaction to generate a Mg-MOF-74 film layer with good bonding strength and good corrosion resistance; the present invention has simple operating steps, environmentally friendly and non-toxic raw materials, and a short time consumption. Only a trace amount of added elements can be used to obtain a better Mg-MOF-74 film layer, and the energy consumption is lower.

[0116] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention.

Claims

1. A method for preparing a Mg-MOF-74 film layer on the surface of a magnesium alloy micro-arc oxidation film. It is characterized in that The steps include: 1) immersing the magnesium alloy in a micro-arc oxidation growth solution for micro-arc oxidation treatment to obtain a magnesium alloy covered with a MAO layer; 2) The magnesium alloy coated with the MAO layer is immersed in an in-situ growth solution for an in-situ solvothermal reaction, and then cleaned and dried to obtain a magnesium alloy coated with a Mg-MOF-74 film layer, i.e., a Mg-MOF-74 film layer on the surface of the magnesium alloy MAO film.

2. The method for preparing the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film according to claim 1, It is characterized in that The micro-arc oxidation growth liquid includes an aqueous solution of 0.03-0.06M trisodium phosphate dodecahydrate and 0.1-0.3M sodium hydroxide.

3. The method for preparing the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film according to claim 2, It is characterized in that The process parameters of the micro-arc oxidation treatment are: the temperature of the micro-arc oxidation growth liquid is 5-10° C., the reaction voltage is 300-400 V, and the reaction time is 2-8 min.

4. The method for preparing the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film according to claim 1, It is characterized in that The in-situ growth solution includes a mixed solution of 0.2-0.4 mM magnesium nitrate and 0.3-0.5 mM trimesic acid; the mixed solution is a mixture of N-, N-dimethylformamide, anhydrous ethanol and deionized water in a volume ratio of 15:1:

1.

5. The method for preparing the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film according to claim 4, It is characterized in that The process parameters of the in-situ solvent thermal reaction are: reaction temperature of 100-140° C., and reaction time of 16-32 h.

6. The method for preparing the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film according to claim 1, It is characterized in that The method also includes pre-treatment of the magnesium alloy before micro-arc oxidation treatment, specifically, grinding the magnesium alloy substrate first, and then degreasing and deoiling the ground magnesium alloy substrate.

7. The method for preparing the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film according to claim 6, It is characterized in that The grinding treatment specifically includes: using 150#, 600#, 800#, 1200#, and 2000# sandpaper to grind the magnesium alloy substrate, and using alcohol to perform ultrasonic cleaning and then drying.

8. The method for preparing the Mg-MOF-74 film layer on the surface of the magnesium alloy micro-arc oxidation film according to claim 6, It is characterized in that The degreasing and oil removal solution used in the degreasing and oil removal process is an aqueous solution including 40 g / L of sodium hydroxide, 25 g / L of sodium carbonate, and 40 g / L of sodium phosphate, based on mass volume concentration.

9. Application of Mg-MOF-74 film layer on the surface of magnesium alloy micro-arc oxidation film prepared by any preparation method of claim 1 to 8 in aerospace, automobile, medical equipment and 3C digital fields.

Citation Information

Patent Citations

  • Compound modified coating of magnesium or magnesium alloy surface carbon-containing nano tube and preparation method of compound modified coating

    CN105274603A

  • Micro-arc oxidation magnesium alloy surface one-step in-situ generated Zn-MOF coating and preparation method thereof

    CN113668035A

  • Preparation and application of multifunctional composite coating for magnesium alloy protection

    CN114774906A

  • Metal-organic framework composite diaphragm, battery comprising same and manufacturing method of metal-organic framework composite diaphragm

    CN115810867A

  • Metal-organic framework catalysts for selective cleavage of aryl-ether bonds

    US9718748B1

Cited By

  • A method for preparing a MOF-74-based polymer membrane synthesized in situ at room temperature

    CN123038691A