Titanium-based hollow electrode and manufacturing method thereof, and photoelectrocatalysis device and method

The porous titanium-based hollow fiber electrode was manufactured through phase conversion method, which solved the problems of short titanium dioxide electron-hole recombination life and limited reaction sites of titanium-based electrodes, and achieved high-efficiency photoelectrocatalysis of titanium-based electrodes, especially the conversion efficiency of methane promote.

CN118910650APending Publication Date: 2024-11-08SHANGHAI ADVANCED RES INST CHINESE ACADEMY OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411037195.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The short electron-hole recombination life of titanium dioxide in the field of photoelectro-catalysis leads to carrier loss, limiting its photo-electric conversion efficiency. The reaction sites of titanium-based electrodes are limited and chemically active, resulting in difficulty in improving efficiency.

Method used

The titanium-based hollow fiber electrode with a porous structure was manufactured by phase conversion method, and the nano-TiO2 structure was grown using titanium hollow fibers, which increased the reaction site and improved conductivity. The sintering and hydrothermal treatment were combined with different substrates and atmospheres to form a loaded titanium acid. The titanium hollow fibers of salt are finally calcined to form a titanium-based hollow electrode.

Benefits of technology

The reaction efficiency is effectively improved, the problems of poor conductivity of TiO2 and insufficient reaction sites are overcome, and the photoelectrocatalytic activity of the titanium-based electrode is enhanced, especially the conversion efficiency of the difficult-to-soluble gas methane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910650A_ABST
    Figure CN118910650A_ABST
Patent Text Reader

Abstract

The invention relates to a method for manufacturing a titanium-based hollow electrode, which comprises the following steps of: manufacturing a titanium hollow fiber green body by a phase inversion method, and roasting in an oxidizing atmosphere at 200-600 DEG C to obtain a first semi-finished product with a semi-stable TiOx layer mixed with carbon residue; sintering the first semi-finished product at 500-1000 DEG C to enable the carbon residues and TiOx to be subjected to a carbon thermal reduction reaction to obtain a second semi-finished product; sintering the second semi-finished product at 1000-1600 DEG C to obtain the titanium hollow fiber; and carrying out hydrothermal reaction on the titanium hollow fiber in an alkaline solution, carrying out immersion cleaning in an acid solution, and then roasting at 300-800 DEG C to obtain the titanium-based hollow electrode of which the surface is loaded with a nano TiO2 structure. The electrode has good strength and photoelectric catalytic reaction efficiency, and can efficiently catalyze and convert methane into n-propanol. The invention further provides a titanium-based hollow electrode, a photoelectrocatalysis device and a photoelectrocatalysis method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of photocatalysis, and specifically relates to a titanium-based hollow electrode and a manufacturing method thereof, and a photoelectric catalytic device and method. Background Art

[0002] Titanium dioxide is one of the most widely used semiconductor photocatalytic materials. It has the advantages of high availability, low cost, good photostability and non-toxicity. Moreover, as a semiconductor material, it has sufficient band gap energy level, so it is widely used in the field of photoelectrocatalysis. However, the short electron-hole recombination lifetime and the carrier loss caused by titanium dioxide limit the light-to-electric conversion efficiency of titanium dioxide. Metal titanium has good electrical conductivity, mechanical strength and chemical stability, and has good photoelectrochemical potential. Therefore, titanium foil or titanium mesh can be used as a substrate at present, and a titanium dioxide layer is formed on the surface of the substrate in the form of mild chemical oxidation to improve the conductivity of titanium dioxide and improve the photocatalytic activity of the material. However, titanium foil or titanium mesh has a small specific surface area and can provide limited reaction sites. Titanium has high chemical activity at high temperature, is easily oxidized, and is easily brittle in a reducing atmosphere, resulting in process difficulties in further improving the efficiency of titanium-titanium oxide composite electrodes through structural optimization. Therefore, it is of positive significance to provide a method for manufacturing a titanium-based electrode with higher reaction efficiency. Summary of the invention

[0003] The purpose of the present invention is to provide a method for manufacturing a titanium-based hollow electrode to improve the reaction efficiency of the titanium-based electrode. The present invention also provides a titanium-based hollow electrode, a photoelectric catalytic device, and a photoelectric catalytic method.

[0004] According to an embodiment of one aspect of the present invention, a method for manufacturing a titanium-based hollow electrode is provided, the method comprising the following steps:

[0005] Step a): using titanium-containing powder, a binder and a dispersant as raw materials to prepare a slurry, and manufacturing the slurry into a titanium hollow fiber green body by a phase inversion method;

[0006] Step b): placing the titanium hollow fiber green body into a corundum tube substrate and calcining at 200°C-600°C in an oxidizing atmosphere to form semi-stable TiO x layer, so that the binder decomposes and at least partially forms a carbon slag mixed in the semi-stable TiO x layer, obtaining a first semi-finished product;

[0007] Step c): transferring the first semi-finished product to a quartz tube substrate and heating it to 500°C-1000°C in an inert atmosphere for sintering, so that the carbon slag and the semi-stable TiO xA carbothermal reduction reaction occurs to obtain a second semi-finished product;

[0008] Step d): transferring the second semi-finished product to a molybdenum tube substrate and heating to 1000° C.-1600° C. in an inert atmosphere for sintering to obtain a titanium hollow fiber;

[0009] Step e): acid-washing the titanium hollow fiber, and then immersing it in an alkaline solution for hydrothermal reaction to obtain a titanium hollow fiber loaded with titanate;

[0010] Step f) transferring the titanium hollow electrode loaded with titanate to an acid solution for immersion and drying to obtain a titanium hollow fiber loaded with titanate nanoarrays;

[0011] Step g): calcining the titanium hollow fiber loaded with titanate nanoarray in air at a temperature of 300°C-800°C to obtain a titanium-based hollow electrode product, wherein the surface of the titanium-based hollow electrode product is loaded with nano-TiO 2 structure.

[0012] This method forms a titanium-based electrode with a porous structure through a phase inversion method, which effectively increases the reaction sites and can solve the problem of limited mass transfer of insoluble gases such as methane. By first preparing titanium hollow fibers, and then growing nano-TiO on the titanium hollow fibers as the substrate 2 The structural approach can effectively overcome the TiO 2 The defect of poor conductivity is improved to improve the reaction efficiency; in the manufacturing process, the electrode semi-finished product is protected by the substrate, which can avoid damage to the brittle electrode semi-finished product, improve the quality of the finished product and reduce the manufacturing cost; the carbon slag left by the decomposition of the binder can effectively reduce the oxide layer on the surface of the titanium-containing powder, avoiding the residual oxide layer on the particle interface of the original titanium-containing powder in the finished electrode to affect the conductivity of the electrode.

[0013] Furthermore, in some embodiments, the weight ratio of the Ti element in the slurry is 50%-70%, the weight ratio of the binder is 5%-15%, and the weight ratio of the dispersant is 20%-40%.

[0014] Furthermore, in some embodiments, the titanium-containing powder is configured as titanium powder, titanium oxide powder or a titanium-containing organic compound; the binder is configured as one or more combinations of polyethersulfone, polyvinylpyrrolidone, polystyrene, polyethyleneimine, polyethylene, polypropylene, polycarbonate or polyamide; the dispersant is configured as one or more combinations of N-methyl-2-pyrrolidone, N,N-dimethylamide or dimethyl sulfoxide.

[0015] Furthermore, in some embodiments, the oxidizing atmosphere in step b) is air, the calcination temperature is 400° C.-600° C., and the calcination time is 5 h-20 h.

[0016] Furthermore, in some embodiments, in the step c), the inert atmosphere is argon, and the heating temperature is 600°C-800°C; in the step d), the inert atmosphere is argon, and the heating temperature is 1200°C-1400°C.

[0017] Further, in some embodiments, in the step e), the pickling is performed with a 0.5M-2M HCl solution; the alkaline solution is performed with a concentration of 1M-5M NaOH, KOH, Na 2 CO 3 or K 2 CO 3 The solution has a hydrothermal reaction temperature of 100°C-250°C and a reaction time of 1h-10h.

[0018] Furthermore, in some embodiments, in the step f), the acid solution is a 0.5M-2M HCl solution.

[0019] Furthermore, in some embodiments, in the step g), the calcination temperature is 400° C.-550° C., and the calcination time is 1 h-5 h.

[0020] According to another embodiment of the present invention, a titanium-based hollow electrode is provided, wherein the electrode comprises a titanium hollow fiber substrate and a nano-TiO 2 layer, and the titanium-based hollow electrode is manufactured by the titanium-based hollow electrode manufacturing method provided in any of the aforementioned embodiments.

[0021] According to an embodiment of another aspect of the present invention, there is provided a photoelectrocatalytic device, comprising a reaction cell, a cathode, and a photoanode, wherein the reaction cell contains an electrolyte, the cathode and the photoanode are respectively at least partially immersed in the electrolyte, the cathode adopts a platinum electrode, and Hg / HgO is used as a reference electrode, and the photoanode adopts the titanium-based hollow electrode provided in the aforementioned embodiment; one end of the titanium-based hollow electrode is externally sheathed with a conductive conduit, and the other end is closed, the conductive conduit is circumferentially bonded to the titanium-based hollow electrode by a conductive adhesive, and the conductive conduit is used to introduce a reaction gas into the titanium-based hollow electrode and provide current; the photoelectrocatalytic device also comprises a light source, and the light source irradiates the photoanode.

[0022] According to another embodiment of the present invention, a photoelectrocatalytic method is provided, which adopts the photoelectrocatalytic device provided in the above embodiment and comprises the following steps: introducing methane into the titanium-based hollow electrode, allowing the methane to diffuse outward through the wall of the titanium-based hollow electrode, and forming a solid-liquid-gas three-phase interface on the surface of the titanium-based hollow electrode; providing light to the titanium-based hollow electrode through the light source; providing current to the titanium-based hollow electrode through the conductive conduit;

[0023] The reaction product of methane is collected. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1a A photo of a titanium hollow fiber in one embodiment;

[0025] Figure 1b This is a cross-sectional photo of a titanium hollow fiber in one embodiment;

[0026] Figure 1c This is a scanning electron microscope photo of the surface of a titanium hollow fiber in an embodiment;

[0027] Figure 1d A photo of a titanium-based hollow electrode in one embodiment;

[0028] Figure 1e A cross-sectional photo of a titanium-based hollow electrode in one embodiment;

[0029] Figure 1f This is a scanning electron microscope photo of the surface of a titanium-based hollow electrode in an embodiment;

[0030] Figure 2 This is a scanning electron microscope photograph of the surface of the first semi-finished product in one embodiment.

[0031] The purpose of the above drawings is to explain the present invention in detail so that those skilled in the art can understand the technical concept of the present invention, but it is not intended to limit the present invention. DETAILED DESCRIPTION

[0032] The present invention is further described in detail below through specific embodiments in conjunction with the accompanying drawings.

[0033] Mentioning "embodiment" herein means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present invention. The phrase appearing in various locations in the specification does not necessarily refer to the same embodiment, nor is it limited to mutually exclusive independent or alternative embodiments. It should be understood by those skilled in the art that the embodiments herein can be combined with other embodiments without structural conflicts. In the description herein, terms such as "first" and "second" are only used to distinguish different objects, and cannot be understood as indicating relative importance or limiting the number, specific order or primary and secondary relationship of the described technical features. In the description herein, the meaning of "multiple" is at least two.

[0034] With the increasing requirements for energy conservation and emission reduction and the increasing environmental pressure, artificial photosynthetic catalytic reactions that directly convert solar energy into chemical energy have been widely studied. 2As the most commonly used semiconductor photocatalyst, TiO has the advantages of high availability, low cost, good photostability and non-toxicity. At the same time, it has sufficient band gap energy level to directly drive the photoelectrocatalytic process. 2 The short electron-hole recombination lifetime leads to significant carrier loss during charge transport, which limits the TiO 2 The low photoelectric conversion efficiency restricts its application as a photoelectric catalytic material. At present, some existing schemes use titanium foil or titanium mesh as the substrate to load TiO on the Ti substrate. 2 The composite electrode is formed by using Ti substrate as TiO 2 Providing a conductive pathway to achieve faster charge transfer, which improves the photoelectrocatalytic efficiency to a certain extent. However, TiO2 loaded on titanium foil or titanium mesh in the form of a thin film 2 The specific surface area of ​​the layer is relatively small, and the reaction sites are relatively insufficient.

[0035] For insoluble gases such as methane, in the process of converting them into chemical raw materials such as ethylene, formic acid or propanol through photoelectrocatalysis, the mass transfer efficiency of methane in the electrolyte is very low due to the low solubility of methane gas. 2 The efficiency is still unable to meet the industrial demand of methane photoelectrocatalytic reaction.

[0036] In order to solve the above problems, an embodiment of one aspect of the present invention provides a method for manufacturing a titanium-based hollow electrode, wherein a Ti / TiO2 having a porous wall is manufactured by a phase transformation method. 2 The composite hollow fiber electrode uses the forced diffusion effect of the hollow fiber electrode to greatly increase the gas mass transfer during the reaction process, shorten the diffusion path of insoluble gases such as methane, and use the porous structure of the hollow fiber electrode to increase the TiO 2 reaction area, effectively improving the efficiency of photoelectrocatalytic reaction.

[0037] The method comprises the following steps:

[0038] Step a): titanium-containing powder, organic polymer binder and organic solvent dispersant are used as raw materials, and are configured into a slurry by ball milling and mixing, and then the slurry is prepared into a titanium hollow fiber green body by phase inversion. In different embodiments, the titanium-containing powder can be titanium powder, titanium oxide powder or an organic compound containing titanium, wherein the titanium-containing organic compound should be able to decompose at high temperature in an oxidizing atmosphere without leaving any other components except titanium; the binder can be one or a combination of polyethersulfone (PES), polyvinylpyrrolidone (PVP), polystyrene (PS), polyethyleneimine (PEI), polyethylene, (PE), polypropylene (PP), polycarbonate (PC) or polyamide (PA); the dispersant can be one or a combination of N-methyl-2-pyrrolidone (NMP), N,N-dimethylamide (DMF), N,N-diethylformamide (DEF) or dimethyl sulfone (DMSO).

[0039] Step b): The titanium hollow fiber green body is loaded into a corundum tube substrate and calcined at 200°C-600°C in an oxidizing atmosphere to form a semi-stable TiO x layer, so that the binder decomposes and carbonizes, and at least in the TiO x The remaining carbon slag is used to obtain the first semi-finished product, which is Ti / TiO x Composite brittle hollow fibers require a corundum tube substrate to provide protection to avoid brittle fracture. The oxidizing atmosphere is a gas environment containing a certain amount of oxygen. In a preferred embodiment, the calcination is carried out in air, the temperature is set at 400°C-600°C, and the calcination time is 8h-20h. Ti is easily oxidized at high temperatures, and TiO x It is not possible to reduce it by heating with reducing gases such as hydrogen. Therefore, the carbon residue of the binder must be retained during the roasting process to be used for the subsequent heating process to reduce the TiO x Reduced to metallic Ti to improve the conductivity of the finished fiber.

[0040] Step c): The first semi-finished product is transferred to a quartz tube substrate, and sintered at 500°C-1000°C in an inert gas to make TiO x The carbon residue and semi-stable TiO x Carbothermal reduction reaction occurs, TiO x The second semi-finished product is a titanium hollow fiber with a porous wall. Since the sintering temperature is relatively low, the brittleness of the second semi-finished product is still obvious. In a preferred embodiment, since nitrogen easily reacts with Ti at high temperature to form TiN, argon is used as the inert gas, the heating temperature is 600°C-800°C, and the heating time is 8h-10h.

[0041] Step d): The second semi-finished product is transferred to a molybdenum tube substrate, and heated to 1000°C-1600°C in an inert gas to obtain a titanium hollow fiber. After high-temperature sintering, the titanium hollow fiber has good strength and toughness, and is not prone to brittle fracture during subsequent processing and use. In a preferred embodiment, the sintering temperature is 1200°C-1400°C, and the sintering time is 2h-5h. x The contact is easily oxidized, and above 1000℃, Ti will react with SiO 2 Therefore, the first semi-finished product needs to be sintered at a lower temperature in a quartz tube to remove the oxygen element through a carbon thermal reduction reaction, and then transferred to a molybdenum tube and sintered at a higher temperature to further sinter and fuse the originally roughly granular titanium structure to enhance the strength of the finished fiber.

[0042] Step e): The titanium hollow fiber is pickled to remove any residual oxide layer on the surface, followed by ultrasonic treatment in acetone, ethanol and deionized water and drying. In a preferred embodiment, a 0.5M-2M hydrochloric acid solution is used for pickling, and sulfuric acid or nitric acid of equivalent concentration may also be used in other embodiments. The dried titanium hollow fiber is immersed in an alkaline solution and heated for hydrothermal reaction to obtain a titanium hollow fiber with titanate loaded on the surface. In different embodiments, the alkaline solution may be KOH, NaOH or K 2 CO 3 、Na 2 CO 3 The reaction temperature is 100℃-250℃ and the reaction time is 1h-10h. Depending on the solute used in the alkaline solution, Na is formed on the surface of the titanium hollow fiber. 2 Ti 2 O 5 ·H 2 O or K 2 Ti 2 O 5 ·H 2 In a preferred embodiment, the reaction temperature of the hydrothermal reaction is 160°C-200°C.

[0043] In different embodiments, by controlling the hydrothermal reaction temperature and the alkaline solution concentration, the growth kinetics of the nanostructure can be affected, thereby controlling the TiO 2The effect of the size and morphology of the precursor (titanate) of the present invention. In one embodiment, the alkaline solution used is a NaOH solution, and the growth of sodium titanate in the NaOH solution mainly includes the dissolution of pure titanium, the diffusion of sodium titanate and the precipitation and crystallization process of sodium titanate. High NaOH concentration, high reaction temperature and longer hydrothermal time will accelerate the growth of nanostructures to obtain thicker nanostructures. In the early stage of the hydrothermal reaction, sodium titanate forms thin and dense nanocrystals on the titanium hollow fiber substrate. As the hydrothermal reaction time increases, the sodium titanate nanocrystals continue to grow, dissolve and diffuse into the NaOH solution. There is a suitable concentration gradient between the titanium hollow fiber and the NaOH solution, thereby forming a hierarchical structure. At low NaOH concentrations (less than 1M), the sodium titanate nanocrystals in contact with the titanium hollow fiber substrate have a lower diffusion rate and accumulate on the Ti surface to form a multidimensional growth, tending to form a nanosheet structure at the bottom. As the NaOH concentration increases (greater than 1M), the yield of sodium titanate is accelerated, the concentration difference becomes smaller, and the sodium titanate tends to grow in a high-dimensional direction. In solutions with higher NaOH concentrations (1-5 M), the yield of sodium titanate is the highest and the diffusion rate is fast, which makes the sodium titanate grow in the same dimension but without uniform orientation, and the nanosheets are completely transformed into nanowires. When the NaOH concentration is further increased to 7-9 M, the morphology of the grown nanowires does not change, but their length and diameter become longer and wider, respectively. After neutralization with HCl solution and annealing, TiO 2 Nanowires. Controlling the hydrothermal temperature and time can also control the growth rate of sodium titanate to achieve different nanostructures. At the same NaOH concentration, amorphous TiO 2 It is formed at low temperature (120℃-140℃) because low temperature cannot provide the energy required to trigger the nucleation of nanosheets. As the temperature increases, it is conducive to the dissolution of the titanium hollow fiber substrate, and small nanosheets with a thickness of 30nm begin to form on the surface of the titanium hollow fiber substrate at 160℃. Therefore, the preferred temperature is greater than 160℃. When the temperature rises to 200℃, the morphology changes dramatically, the disordered flakes disappear, and the energy provided by the hydrothermal reaction transforms the thin nanosheets into nanowires. The higher the reaction temperature, the more energy is provided, which promotes the dissolution of the titanium hollow fiber substrate, which may promote the formation of crystalline nanowires. The nanowires actually undergo a secondary crystallization process at high temperatures, thereby increasing the TiO 2Crystallinity of nanowires. When the temperature is further increased to 240°C, the nanowires on the titanium hollow fiber substrate grow further and begin to "meet" at the top. The longer nanowires self-assemble into a macroporous scaffold on the titanium hollow fiber substrate. In addition, longer reaction times will produce longer nanowires that can bend at the top and begin to self-assemble with each other, rather than remaining vertical and growing randomly. In a 1M concentration NaOH solution, wrinkled nanosheets are formed within 1h, and when the reaction time is increased to 2h, the nanosheets gradually transform into loosely stacked and porous nanowires. More nanowires can be produced over time.

[0044] Step f): transferring the titanium hollow electrode loaded with titanate to an acid solution for immersion and drying to obtain a titanium hollow electrode loaded with titanate (H 2 Ti 2 O 5 ·H 2 O) Titanium hollow fiber of nano-array In a preferred embodiment, the acid solution is a 0.5M-2M hydrochloric acid solution, and in a gas embodiment, sulfuric acid or nitric acid of equivalent concentration may also be used.

[0045] Step g): The titanium hollow fiber loaded with titanate nanoarray after acid washing is transferred to a muffle furnace for calcination in air to obtain a titanium hollow fiber loaded with nano-TiO 2 In some embodiments, the calcination temperature is 300°C-800°C. When the calcination temperature is greater than 550°C, TiO 2 The crystal form tends to change from anatase to rutile, and because rutile TiO 2 The photogenerated electrons and holes under light excitation are more likely to recombine, which is not conducive to the photoelectrocatalytic reaction. Therefore, in the preferred embodiment, the calcination temperature is 400°C-550°C and the calcination time is 1h-5h to obtain anatase TiO with better photocatalytic activity. 2 .

[0046] The titanium-based hollow electrode manufactured by the method provided in the above embodiment has titanium hollow fiber as the matrix, and nano-TiO 2 The hollow fiber wall is porous, which allows methane and other gases to diffuse through the wall and form a solid-liquid-gas three-phase interface on the electrode surface, effectively increasing the reaction area while shortening the mass transfer distance. The titanium hollow fiber matrix effectively improves the TiO 2 The conductivity of the material can effectively improve the efficiency of the photoelectrocatalytic reaction, especially the photoelectrocatalytic reaction of insoluble gases such as methane.

[0047] According to another embodiment of the present invention, there is provided a photoelectrocatalytic device, which includes a reaction cell, wherein the reaction cell contains an electrolyte, and the device uses the titanium-based hollow electrode provided in the above embodiment as a photoanode, a platinum electrode as a cathode, Hg / HgO as a reference electrode, and provides a light source capable of irradiating the photoanode. One end of the titanium-based hollow electrode is sealed with epoxy resin, and the other end is sheathed with a conductive conduit outside the electrode. The conductive conduit and the titanium-based hollow electrode are circumferentially bonded and sealed with conductive glue, so that the conductive conduit can transport the reacting gas raw material into the titanium-based hollow electrode and energize it. The photoanode and the cathode are at least partially immersed in the electrolyte, respectively. In different embodiments, the light source uses sunlight or other artificial light sources, and can be in different forms such as top lighting or side lighting according to the different structures of the reaction cell. According to the specific structure of the photoelectrocatalytic device, the photoanode can be set as a single one, or it can be set as a row or array composed of multiple electrodes.

[0048] In one embodiment, during operation, the photoelectrocatalytic device introduces methane into the titanium-based hollow electrode, allowing the methane to diffuse outward through the wall of the titanium-based hollow electrode and form a solid-liquid-gas three-phase interface on the surface of the titanium-based hollow electrode; while the titanium-based hollow electrode is irradiated by a light source, the titanium-based hollow electrode is powered by a conductive conduit to drive the photoelectrocatalytic reaction. The reaction products of methane are collected and detected, and depending on the specific reaction conditions, the reaction products include n-propanol and the like.

[0049] In a preferred embodiment, a plurality of groups of titanium-based hollow electrodes are manufactured by the following method, and a photoelectrocatalytic reaction of methane is carried out using a photoelectrocatalytic device equipped with these titanium-based hollow electrodes.

[0050] First, spherical titanium powder, NMP, and PES were used as raw materials, mixed and ball-milled at a speed of 300 r / min for 24 hours to obtain a slurry, and the proportions of each component are shown in Table 1. A higher titanium powder particle concentration was selected during the manufacturing process to reduce shrinkage and anisotropic deformation during the subsequent sintering process. After ball milling, the slurry was placed in a vacuum drying oven for 12 hours for vacuum degassing.

[0051]

[0052] Table 1 Titanium hollow fiber manufacturing parameters

[0053] Subsequently, the green body was prepared by phase inversion method. A spinning head with a size of Φ34×1.0×0.3mm was used, ultrapure water was used as the core liquid, the slurry liquid (casting liquid) flow rate was controlled to be 5mL / min, the core liquid flow rate was 8mL / min, water was used as the coagulation liquid, and the air distance between the spinning head and the coagulation liquid surface was controlled to be 1cm to prepare the titanium hollow fiber green body. The titanium hollow fiber green body was soaked in water for 24 hours to remove excess solvent, and was shaped and dried for 48 hours under ambient conditions.

[0054] Next, the titanium hollow fiber green body was loaded into the quartz tube substrate, and the air flow rate was controlled to be 200 mL / min and the heating rate was 2°C / min for calcination to decompose the PES as a binder to obtain the first semi-finished product. The calcination temperature and time are shown in Table 1. Figure 2 As shown in Figure 2, during the calcination process, the Ti on the surface undergoes controlled oxidation to form semi-stable TiO x Layer 1 (gray spherical structure in SEM image), while PES is partially carbonized to form a mixture of semi-stable TiO x Carbon residue in the layer (TiO x bright areas at the edges).

[0055] Next, the first semi-finished product was transferred to the corundum tube substrate, and the argon flow rate was adjusted to 200 mL / min and the heating rate was 4 °C / min for sintering to make the carbon slag and the semi-stable TiO x The layer undergoes a carbothermal reduction reaction to obtain a second semi-finished hollow fiber product having a component of Ti. The specific sintering temperature and time are shown in Table 1.

[0056] The second semi-finished product was transferred to the molybdenum tube substrate, and the argon flow rate was controlled to 200 mL / min and the heating rate was 8 °C / min, so that the metal titanium particles were further sintered and connected together to obtain a titanium hollow fiber with good strength and conductivity. The specific sintering temperature and time are shown in Table 1. Its macroscopic appearance is as follows Figure 1a As shown, the cross-sectional morphology is Figure 1b The surface microstructure is shown in Figure 1c shown.

[0057] Next, the titanium hollow fiber is chemically modified to form uniformly grown nano-TiO 2 Structural layer.

[0058] sample Type and concentration of hydrothermal solution Hydrothermal temperature / time Calcination temperature / heating rate / holding time <![CDATA[TiO 2 Nanostructures]]> Example 1 NaOH 1M 200℃ / 2h 450℃ / 2℃ / min / 2h Nanowires Example 2 NaOH 1M 200℃ / 2h 450℃ / 2℃ / min / 2h Nanowires Example 3 NaOH 1M 200℃ / 2h 450℃ / 2℃ / min / 2h Nanowires Example 4 KOH 1M 180℃ / 5h 450℃ / 1℃ / min / 2h Nanosheets Example 5 NaOH 1M 160℃ / 2h 500℃ / 2℃ / min / 2h Nanosheets Example 6 NaOH 1M 240℃ / 5h 500℃ / 5℃ / min / 5h Nanowires Example 7 NaOH 1M 200℃ / 5h 450℃ / 2℃ / min / 5h Nanowires Example 8 NaOH 1M 200℃ / 10h 550℃ / 2℃ / min / 2h Nanowires Example 9 NaOH 1M 200℃ / 10h 550℃ / 2℃ / min / 5h Nanowires Example 10 NaOH 1M 200℃ / 2h 450℃ / 2℃ / min / 2h Nanowires

[0059] Table 2 Nano-TiO 2 Preparation conditions of the structure

[0060] The titanium hollow fiber was ultrasonically treated in 1M HCl solution for 15 min to remove the possible surface oxide layer, and then ultrasonically treated in acetone, ethanol and deionized water for 15 min respectively, and then fully dried in air. Next, the titanium hollow fiber was immersed in an alkaline solution for hydrothermal treatment to form in situ growth TiO on the surface of the titanium hollow fiber. 2 The precursor (titanate), solute, concentration and hydrothermal treatment conditions of the alkaline solution are shown in Table 2.

[0061] The hydrothermally treated titanium hollow fiber was immersed in a 1M HCl solution for 10 min to allow the H in the solution to+ Substituting metal particles in titanate to form H 2 Ti 2 O 5 ·H 2 O nanoarray.

[0062] Finally, the load has H 2 Ti 2 O 5 ·H 2 The titanium hollow fiber with O nanoarray was transferred to a muffle furnace for calcination to make H 2 Ti 2 O 5 ·H 2 O is transformed into uniform nano-TiO 2 The structure of the finished titanium-based hollow electrode was obtained. Calcination conditions and TiO formed under different hydrothermal treatment conditions 2 The nanostructure is shown in Table 2. The macroscopic morphology of the finished titanium-based hollow electrode is shown in Figure 1d Its cross-sectional morphology is shown in Figure 1e As shown, the nanowire structure TiO 2 The surface microstructure of the titanium-based hollow electrode is as follows Figure 1f shown.

[0063] The single titanium-based hollow electrode provided in the above embodiment is used as a photoanode, and the platinum electrode is used as a cathode. The electrodes are immersed in an electrolytic cell to form a photoelectrochemical catalytic device. One end of the photoanode is closed, and the other end is inserted into a copper tube and circumferentially bonded with a conductive adhesive. Methane is introduced into the photoanode through the copper tube to force methane to penetrate the porous wall of the photoanode into the electrolyte, forming a gas-liquid-solid three-phase interface on the surface of the photoanode. The device is used to carry out the photocatalytic reaction of methane under different conditions as shown in Table 3.

[0064] sample Catalytic method Electrolyte type and concentration Electrolysis conditions n-Propanol selectivity n-Propanol yield Example 1 photoelectric KOH 1M <![CDATA[10mA cm -2 ]]> 99% <![CDATA[~20μmol g cat -1 h -1 ]]> Example 2 Light KOH 1M ~ 99% <![CDATA[~10μmol g cat -1 h -1 ]]> Example 3 electricity KOH 1M <![CDATA[10mA cm -2 ]]> ~ ~ Example 4 photoelectric <![CDATA[Na 2 CO 3 1M]]> <![CDATA[10mA cm -2 ]]> 85% <![CDATA[~5μmol g cat -1 h -1 ]]> Example 5 photoelectric KOH 2M <![CDATA[10mA cm -2 ]]> 99% <![CDATA[~25μmol g cat -1 h -1 ]]> Example 6 photoelectric KOH 5M <![CDATA[10mA cm -2 ]]> 99% <![CDATA[~26μmol g cat -1 h -1 ]]> Example 7 photoelectric KOH 0.5M <![CDATA[10mA cm -2 ]]> 99% <![CDATA[~15μmol g cat -1 h -1 ]]> Example 8 photoelectric KOH 1M <![CDATA[500mA cm -2 ]]> 50% <![CDATA[~100μmol g cat -1 h -1 ]]> Example 9 photoelectric KOH 1M <![CDATA[100mA cm -2 ]]> 80% <![CDATA[~50μmol g cat -1 h -1 ]]> Example 10 photoelectric KOH 1M <![CDATA[50mA cm -2 ]]> 90% <![CDATA[~20μmol g cat -1 h -1 ]]>

[0065] Table 3 Results of methane catalytic reaction under different conditions

[0066] It can be seen that when only current is applied, the device has no output; however, when only light is applied or light and electricity are applied, the device can efficiently convert methane into n-propanol with a selectivity of not less than 50%. -2 Under the current conditions, the selectivity of n-propanol can reach 99%.

[0067] The manufacturing and sintering process of titanium hollow fiber green body can control the pore size of titanium hollow fiber by optimizing the particle size of spherical Ti powder and the sintering temperature, heating rate and holding time of titanium hollow fiber. The smaller the particle size of spherical Ti powder, the higher the sintering temperature of titanium hollow fiber, the longer the calcination time, and the smaller the pore size of the final titanium hollow fiber. Since TiO 2 Nanostructure, during hydrothermal treatment, TiO 2 It will not only grow on the surface, but also in the pores of the titanium hollow fiber, which may block the pores. Therefore, it is necessary to select titanium hollow fibers with appropriate pore sizes and suitable TiO 2 growth conditions to obtain suitable CH 4 The breathable length is suitable for TiO 2 Hollow fiber photoanode with nanometer photocatalyst film thickness.

[0068] The catalytic ability of the titanium-based hollow fiber photoanode provided in the above embodiment is similar to that of TiO 2 When TiO 2 When the nanowires are completely covered on the titanium hollow fiber, higher photoelectric activity can be obtained. 2 When the thickness of the nanostructure layer exceeds a certain value, the activity of the photoanode will decrease. This is because the thicker the TiO 2 The layer will affect the electron transport. Therefore, it is necessary to control the reaction conditions to produce TiO with appropriate thickness. 2 Nanostructured layer.

[0069] In addition, the hydrothermal process affects the growth kinetics of TiO due to the concentration of alkaline solution, hydrothermal temperature and time. 2 Defect types and concentrations in nanostructures. TiO grown rapidly in highly concentrated alkaline solutions and hydrothermally 2 There are more defects. The defects include surface oxygen vacancies and bulk oxygen vacancies. These defects are related to the titanium hollow fiber and TiO 2 The Ti atoms at the interface of the nanostructure can act as active sites in the photoelectric activation of methane. The adsorption of reactants and the stabilization and coupling processes of related intermediates are closely related to the active sites. By controlling the hydrothermal temperature and time, the growth of TiO 2The defect concentration of the nanostructure further regulates the adsorption of the intermediate and promotes the coupling process, which can achieve the selective regulation of n-propanol. Among them, the surface oxygen vacancies and the active sites of the interfacial Ti atoms can effectively adsorb and stabilize the *CO intermediate. The *CO intermediate stabilized on the surface oxygen vacancies can be effectively coupled to the *COCO intermediate and transferred to the active sites of the interfacial Ti atoms to stabilize the coupling of the *CO intermediate to form the *COCOCO intermediate, and then form n-propanol through subsequent steps. Rapid growth of TiO by high hydrothermal temperature and high concentration solution 2 , which can effectively improve TiO 2 The oxygen vacancy concentration is increased, thereby increasing the stable *COCO concentration. The synergistic effect of surface oxygen vacancies and interfacial Ti atomic active sites achieves highly selective n-propanol production.

[0070] The methane photoelectric activation process requires firstly to trigger the photoexcitation of the hydroxyl (OH-) in the water / solution to split to produce active oxygen species, which are used to further activate the CH bonds of methane to achieve the subsequent reaction process. Therefore, high concentration KOH is more beneficial for methane activation and product generation (as shown in Examples 2, 5 and 6).

[0071] In addition, products were generated in Example 2 (light was applied but no voltage was applied), but no products were generated in Example 3 (electricity was applied but no light was applied), indicating that methane was generated in the presence of TiO 2 Photoelectric activation on the nanostructured titanium hollow fiber photoanode is generated by light excitation, and methane cannot be activated and converted under pure voltage conditions. Voltage / current density only plays a role in promoting the spatial separation of photogenerated electrons and holes. Since the oxygen evolution reaction of water oxidation and methane oxidation are competitive reactions, under higher applied current density, in Examples 8, 9 and 10, although the activity of methane conversion under high voltage / current density is improved to produce more n-propanol, the oxygen evolution reaction becomes more serious, resulting in a decrease in the selectivity of n-propanol.

[0072] The method for manufacturing a titanium-based hollow electrode provided in the above embodiment can be used to manufacture Ti / TiO with good mechanical strength and photoelectrocatalytic efficiency. 2 The composite electrode improves the conductivity of the electrode, increases the reaction sites, and effectively improves the reaction efficiency of the photoelectrocatalytic process. In particular, for insoluble gas raw materials such as methane, a three-phase reaction interface can be formed through the forced diffusion of the hollow electrode, thereby improving the catalytic efficiency and shortening the mass transfer distance. The photoelectrocatalytic device manufactured using the titanium-based hollow fiber electrode can efficiently convert methane into n-propanol, improve the photoelectrocatalytic utilization efficiency of methane, and reduce the cost of industrialization.

[0073] The purpose of the above embodiments is to further explain the present invention in detail in conjunction with the accompanying drawings so that those skilled in the art can understand the technical concept of the present invention. Within the scope of the present invention, the optimization or equivalent replacement of the method steps or part structures involved, and the combination of the implementation methods in different embodiments without conflict of structure and principle, all fall within the protection scope of the present invention.

Claims

1. A method for manufacturing a titanium-based hollow electrode, characterized in that: The following steps are involved: Step a): using titanium-containing powder, a binder and a dispersant as raw materials to prepare a slurry, and manufacturing the slurry into a titanium hollow fiber green body by a phase inversion method; Step b): placing the titanium hollow fiber green body into a corundum tube substrate and calcining at 200°C-600°C in an oxidizing atmosphere to form semi-stable TiO x layer, so that the binder decomposes and at least partially forms a carbon slag mixed in the semi-stable TiO x layer, obtaining a first semi-finished product; Step c): transferring the first semi-finished product to a quartz tube substrate and heating it to 500°C-1000°C in an inert atmosphere for sintering, so that the carbon slag and the semi-stable TiO x A carbothermal reduction reaction occurs to obtain a second semi-finished product; Step d): transferring the second semi-finished product to a molybdenum tube substrate and heating to 1000° C.-1600° C. in an inert atmosphere for sintering to obtain a titanium hollow fiber; Step e): acid-washing the titanium hollow fiber, and then immersing it in an alkaline solution for hydrothermal reaction to obtain a titanium hollow fiber loaded with titanate; Step f) transferring the titanium hollow electrode loaded with titanate to an acid solution for immersion and drying to obtain a titanium hollow fiber loaded with titanate nanoarrays; Step g): calcining the titanium hollow fiber loaded with titanate nanoarray in air at a calcination temperature of 300°C-800°C to obtain a titanium-based hollow electrode product, the surface of which is loaded with nano-TiO2 structure.

2. The method for manufacturing a titanium-based hollow electrode according to claim 1, characterized in that: The weight ratio of the Ti element in the slurry is 50%-70%, the weight ratio of the binder is 5%-15%, and the weight ratio of the dispersant is 20%-40%.

3. The method for manufacturing a titanium-based hollow electrode according to claim 1 or 2, characterized in that: The titanium-containing powder is configured as titanium powder, titanium oxide powder or a titanium-containing organic compound; the binder is configured as one or more combinations of polyethersulfone, polyvinyl pyrrolidone, polystyrene, polyethyleneimine, polyethylene, polypropylene, polycarbonate or polyamide; the dispersant is configured as one or more combinations of N-methyl-2-pyrrolidone, N,N-dimethylamide or dimethyl sulfoxide.

4. The method for manufacturing a titanium-based hollow electrode according to claim 1, characterized in that: In the step b), the oxidizing atmosphere is air, the calcination temperature is 400° C.-600° C., and the calcination time is 5 h-20 h.

5. The method for manufacturing a titanium-based hollow electrode according to claim 1 or 4, characterized in that: In the step c), the inert atmosphere is argon, and the heating temperature is 600°C-800°C; in the step d), the inert atmosphere is argon, and the heating temperature is 1200°C-1400°C.

6. The method for manufacturing a titanium-based hollow electrode according to claim 1, characterized in that: In the step e), the acid wash uses a 0.5M-2M HCl solution; the alkaline solution uses a 1M-5M NaOH, KOH, Na2CO3 or K2CO3 solution, the temperature of the hydrothermal reaction is 100°C-250°C, and the reaction time is 1h-10h.

7. The method for manufacturing a titanium-based hollow electrode according to claim 1 or 6, characterized in that: In the step f), the acid solution is a 0.5M-2M HCl solution.

8. The method for manufacturing a titanium-based hollow electrode according to claim 1, characterized in that: In the step g), the calcination temperature is 400° C.-550° C., and the calcination time is 1 h-5 h.

9. A titanium-based hollow electrode, characterized in that: It comprises a titanium hollow fiber substrate and a nano-TiO2 layer, and the titanium-based hollow electrode is manufactured by the manufacturing method of the titanium-based hollow electrode according to any one of claims 1 to 8.

10. A photoelectrocatalytic device, characterized in that: The invention comprises a reaction cell, a cathode, and a photoanode, wherein the reaction cell contains an electrolyte, the cathode and the photoanode are respectively at least partially immersed in the electrolyte, the cathode adopts a platinum electrode, and Hg / HgO is used as a reference electrode, and the photoanode adopts the titanium-based hollow electrode as claimed in claim 9; a conductive conduit is externally sheathed at one end of the titanium-based hollow electrode, and the other end is closed, the conductive conduit is circumferentially bonded to the titanium-based hollow electrode by a conductive adhesive, and the conductive conduit is used to pass a reaction gas into the titanium-based hollow electrode and provide current; the photoelectrocatalytic device also comprises a light source, and the light source irradiates the photoanode.

11. A photoelectrocatalytic method, characterized in that: The photoelectrocatalytic device according to claim 10 is used, and comprises the following steps: Introducing methane into the titanium-based hollow electrode, allowing the methane to diffuse outward through the wall of the titanium-based hollow electrode, and forming a solid-liquid-gas three-phase interface on the surface of the titanium-based hollow electrode; Providing illumination to the titanium-based hollow electrode by means of the light source; supplying electric current to the titanium-based hollow electrode through the conductive conduit; The reaction product of methane is collected.