Ho-MOF modified alpha-Fe2O3 photo-anode catalyst as well as preparation method and application thereof
By modifying the surface of the α-Fe2O3 photoanode with Ho-MOF, the problems of electron-hole recombination and photocorrosion were solved, the photoelectric conversion efficiency and stability were improved, and a highly efficient photoelectrocatalytic water oxidation reaction was achieved.
Patent Information
- Application Number
- CN202410966773.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-18
AI Technical Summary
Existing α-Fe2O3 photoanodes suffer from electron-hole recombination and photocorrosion problems in the photoelectrochemical water splitting process for hydrogen production, resulting in low solar energy conversion efficiency and insufficient photostability, making it difficult to meet industrial requirements.
By modifying the surface of α-Fe2O3 photoanode with Ho-MOF and employing specific ligands and solution treatment methods, a Ho-MOF/α-Fe2O3 composite photoanode is formed, which improves the separation of photogenerated carriers and reaction kinetics.
It significantly improved the photocurrent density, reaching 0.57 mA cm⁻², which is 3.56 times higher than that of the pure α-Fe₂O₃ photoanode. Moreover, the photocurrent density showed excellent stability with no significant degradation within 10 minutes.
Smart Images

Figure CN118910671A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of photoelectrocatalytic materials, and in particular to a Ho-MOF-modified α-Fe2O3 photoanode catalyst and a preparation method and application thereof. Background Art
[0002] Photoelectrochemical water splitting to produce hydrogen is an economical and environmentally friendly way to solve the global fossil energy depletion and environmental problems. PEC cells, which simulate photosynthesis in nature, can efficiently and cheaply convert sunlight into chemical fuels. However, due to the low efficiency of solar energy to hydrogen conversion, PEC cells are still far from practical application. Semiconductor photoelectrodes play a vital role in PEC cells. They collect solar energy and convert the absorbed sunlight into photoexcited carriers to drive the PEC water splitting reaction. So far, people have made a lot of efforts and made great progress in developing efficient and stable semiconductor photoelectrodes. Among the semiconductors studied, hematite (α-Fe2O3) is widely regarded as the best candidate material for efficient PEC hydrogen production due to its suitable band gap and flat band potential. However, α-Fe2O3 photoanode has serious defects such as electron-hole recombination and photocorrosion in photoelectrochemical water splitting, which hinders the conversion efficiency of solar energy to hydrogen energy and affects its industrialization. Therefore, improving the photoelectric conversion efficiency and stability of α-Fe2O3 photoanode is the focus of research on anode catalysts for photoelectrochemical cells. Although some progress has been made in the modification of α-Fe2O3 photoanodes, their photocurrent density and photostability still cannot meet the requirements of industrialization. Therefore, it is imperative to research and develop α-Fe2O3 composite photoanodes with higher photocurrent density and better stability.
[0003] Metal organic frameworks (MOFs) are composed of metal nodes and organic connectors, with porous structures and high specific surface areas, which give them good adsorption and catalytic properties. It has been reported that the composite MOFs on the surface of α-Fe2O3 photoanode to form a passivation layer can effectively improve the slow water oxidation kinetics and photocorrosion of α-Fe2O3 (DOI: 10.1021 / acscatal.8b03233). In addition, some articles have reported that doping rare earth metal ions on the catalyst can provide more active sites and effectively improve the catalytic activity (DOI: 10.1002 / aenm.202203244). Among many rare earth metals, holmium, as one of the most catalytically active catalysts, has attracted much attention from researchers. Its characteristics such as stability in air and easy oxidation at high temperatures also meet the standards of industrialization; however, the catalytic performance of the above materials is still not very ideal. Summary of the invention
[0004] The technical problem to be solved by the present invention is how to improve the photocurrent density and photostability of α-Fe2O3 photoanode catalyst.
[0005] The present invention solves the above technical problems through the following technical means:
[0006] A method for preparing a Ho-MOF modified α-Fe2O3 photoanode catalyst comprises the following steps:
[0007] S1. Generate β-FeOOH on FTO conductive glass to obtain FTO / β-FeOOH photoelectrode; anneal the FTO / β-FeOOH photoelectrode in air atmosphere to obtain FTO / α-Fe2O3 photoanode;
[0008] S2, formic acid, N, N-dimethylformamide, ethanol, chiral H3L ligand and holmium salt are mixed uniformly to form a precursor solution; wherein the chiral H3L ligand has a structural formula of The mass ratio of the holmium salt to the chiral H3L ligand is 0.95 g:156-350 mg;
[0009] S3, placing the FTO / α-Fe2O3 photoanode and the precursor solution in a hydrothermal reaction device, sealing it and reacting it, and cooling it after the reaction to obtain the Ho-MOF modified α-Fe2O3 photoanode catalyst.
[0010] Preferably, in S1, the annealing temperature is 500° C. and the time is 2 h.
[0011] Preferably, in S2, the volume ratio of ethanol to N,N-dimethylformamide is 2.5:8-25.
[0012] Preferably, in S2, the mass volume ratio of the chiral H3L ligand to ethanol is 156-350 mg:2.5 ml.
[0013] Preferably, in S2, the ratio of the amount of the holmium salt to the chiral H3L ligand is 0.95 g:156-312 mg.
[0014] Preferably, in S2, the concentration of the chiral H3L ligand in the precursor solution is 5.5-39 mg / ml.
[0015] Preferably, in S3, the reaction temperature is 110-140°C and the reaction time is 12-16h.
[0016] Preferably, in S2, the usage ratio of formic acid and chiral H3L ligand is 0.05-0.1 ml: 156-350 mg; excessive formic acid will affect the growth of MOF.
[0017] Preferably, in S1, ferric chloride, sodium nitrate, concentrated hydrochloric acid and water are used as raw materials, which are mixed and then subjected to a hydrothermal reaction to generate β-FeOOH on the FTO conductive glass.
[0018] Preferably, the mass ratio of the ferric chloride used in S1 to the mass ratio of the chiral H3L ligand used in S2 is 0.6-0.7 g:156-350 mg.
[0019] Preferably, in S1, the following steps are specifically included: mixing ferric chloride, sodium nitrate, concentrated hydrochloric acid and water to form a mixed solution; transferring the mixed solution and FTO conductive glass to a hydrothermal reaction device, sealing and reacting; cooling to room temperature after the reaction is completed, and washing, drying and annealing the obtained product in an air atmosphere to obtain the FTO / α-Fe2O3 photoanode.
[0020] Preferably, in S1, after annealing, the process further includes using an ozone cleaner to obtain a FTO / α-Fe2O3 photoanode.
[0021] Preferably, in S2, the holmium salt is holmium chloride.
[0022] The present invention also provides a Ho-MOF modified α-Fe2O3 photoanode catalyst, which is prepared by using the preparation method of the Ho-MOF modified α-Fe2O3 photoanode catalyst.
[0023] The present invention also proposes an application of the Ho-MOF modified α-Fe2O3 photoanode catalyst as a photoelectrocatalyst for catalyzing water oxidation reaction.
[0024] The FTO conductive glass in the present invention is fluorine-doped SnO2 conductive glass (SnO2:F), referred to as FTO for short.
[0025] The advantages of the present invention are:
[0026] The method of the present invention has the advantages of simple process, low cost, good repeatability, uniform morphology and size of the product, and the prepared Ho-MOF modified α-Fe2O3 photoanode, i.e., α-Fe2O3 / Ho-MOF composite photoanode, has a high conductivity at 1.23V. RHE The photocurrent density under bias voltage reached 0.57 mA cm -2 , which is 3.56 times that of pure α-Fe2O3 photoanode. After systematic testing and characterization studies, the designed Ho-MOF co-catalyst can not only act as a hole extraction layer to promote the separation of photogenerated carriers, but also accelerate the ability of hole injection into the electrolyte to accelerate the reaction kinetics. As a catalyst, it exhibits excellent catalytic performance in the photoelectrocatalytic water oxidation reaction. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1A high-resolution scanning electron microscope (SEM) image of the Ho-MOF-modified α-Fe2O3 photoanode catalyst and the α-Fe2O3 photoanode obtained in Example 1 of the present invention;
[0028] Figure 2 This is a surface scanning element distribution map (Mapping) of the Ho-MOF modified α-Fe2O3 photoanode catalyst obtained in Example 1 of the present invention; wherein af corresponds to the surface scanning area map, the element distribution map of Fe, N, O, C, and Ho, respectively;
[0029] Figure 3 This is an element content analysis diagram of the surface scanning element distribution diagram of the Ho-MOF modified α-Fe2O3 photoanode catalyst obtained in Example 1 of the present invention;
[0030] Figure 4 This is the X-ray photoelectron spectrum (XPS) of the Ho-MOF modified α-Fe2O3 photoanode catalyst obtained in Example 1 of the present invention;
[0031] Figure 5 The X-ray diffraction spectrum (XRD) of the Ho-MOF modified α-Fe2O3 photoanode catalyst and α-Fe2O3 photoanode obtained in Example 1 of the present invention;
[0032] Figure 6 The infrared spectrum of the Ho-MOF modified α-Fe2O3 photoanode catalyst obtained in Example 1 of the present invention and the Fourier infrared spectrum (FTIR) of the α-Fe2O3 photoanode catalyst;
[0033] Figure 7 The LSV curves of the Ho-MOF modified α-Fe2O3 photoanode catalyst and the α-Fe2O3 photoanode in 1M NaOH solution obtained in Example 1 of the present invention; wherein the α-Fe2O3 photoanode is a standard catalyst;
[0034] Figure 8 IT curves of the Ho-MOF modified α-Fe2O3 photoanode catalyst and the α-Fe2O3 photoanode in 1M NaOH solution obtained in Example 1 of the present invention, wherein the α-Fe2O3 photoanode is a standard catalyst;
[0035] Fig. 9 This is a comparison diagram of the LSV curves of the La-MOF-modified α-Fe2O3 photoanode catalyst obtained in Comparative Example 3 of the present invention and the Ho-MOF-modified α-Fe2O3 photoanode catalyst obtained in Example 1;
[0036] Fig.10 This is a schematic diagram of the preparation method of Example 1 of the present invention;
[0037] Fig.11This is a high-resolution scanning electron microscope (SEM) image of the La-MOF-modified α-Fe2O3 photoanode catalyst obtained in Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.
[0040] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0041] The chiral H3L ligand in the following examples and comparative examples is the chiral ligand H3L disclosed in the Chinese patent application document with publication number CN113354556A, and its structural formula is The method for synthesizing the H3L ligand refers to the Chinese patent application document with publication number CN113354556A.
[0042] In the following examples and comparative examples, the pretreated FTO glass was prepared according to the following process: the FTO glass was placed in an ultrasonic cleaner, and cleaned with acetone, ethanol and ultrapure water for a total of 30 minutes, repeatedly cleaned with deionized water and blown dry with nitrogen, and then placed in a clean oven for drying.
[0043] Example 1
[0044] Reference Fig.10 , a method for preparing a Ho-MOF modified α-Fe2O3 photoanode catalyst, comprising the following steps:
[0045] 3.5 g FeCl3·6H2O and 3 g NaNO3 were dissolved in 50 ml deionized water to form a mixed aqueous solution, and 0.15 ml concentrated hydrochloric acid was added to the mixed aqueous solution, and stirred for 15 min to obtain a precursor solution; the pretreated FTO glass conductive surface was placed downward in a polytetrafluoroethylene reactor, and 10 ml of the precursor solution was added along the inner wall of the polytetrafluoroethylene reactor, and the reactor was sealed with a stainless steel hydrothermal reactor, and reacted at 100 ° C for 24 h. After the reaction was completed, it was cooled to room temperature, and the obtained product was washed and dried with a mixed solution of N, N-dimethylformamide and ethanol, and then air annealed at 500 ° C for 2 h in a tube furnace, and then treated with an ozone cleaner for 10 min to obtain an α-Fe2O3 photoanode.
[0046] Modification of Ho-MOF:
[0047] (1) Dissolve 0.95 g of HoCl3·6H2O in 15 ml of DMF solvent to form a metal salt solution;
[0048] (2) 7.5 mL of N,N-dimethylformamide solution (DMF) and 2.5 mL of anhydrous ethanol solution were mixed evenly, and then 156 mg of chiral H3L ligand was added, and the mixture was stirred and ultrasonically mixed to obtain a mixed solution;
[0049] (3) adding the metal salt solution obtained in step (1) to the mixed solution obtained in step (2), and then adding 0.1 ml of formic acid;
[0050] (4) placing the conductive surface of the α-Fe2O3 photoanode facing downward in a polytetrafluoroethylene reactor, and then injecting the solution obtained in step (3) along the non-conductive surface of the α-Fe2O3 photoanode, sealing it with a stainless steel hydrothermal reactor, reacting it at 125°C for 14 hours, and obtaining Ho-MOF after cooling. The obtained product was washed three times with a mixed solution of N,N-dimethylformamide and ethanol, and dried at 60°C to obtain a Ho-MOF-modified α-Fe2O3 photoanode catalyst.
[0051] Figure 1 The high-resolution scanning electron microscope (SEM) images of the Ho-MOF-modified α-Fe2O3 photoanode catalyst (right image) and the α-Fe2O3 photoanode catalyst (i.e., α-Fe2O3 photoanode, left image) obtained in Example 1 of the present invention are shown; Figure 1 It can be seen that the product obtained in this example has a heterogeneous structure and uniform morphology;
[0052] Figure 2 This is the surface scanning element distribution map (Mapping) of the Ho-MOF modified α-Fe2O3 photoanode catalyst obtained in Example 1. Figure 3The element content analysis diagram of the surface scanning element distribution diagram of the Ho-MOF modified α-Fe2O3 photoanode catalyst obtained in Example 1 (the SEM image of the surface scanning area is as follows Figure 2 a); Figures 2-3 It can be seen that the product obtained in this example successfully loaded Ho-MOF.
[0053] Figure 4 This is the X-ray photoelectron spectrum (XPS) of the Ho-MOF-modified α-Fe2O3 photoanode catalyst obtained in Example 1 of the present invention, which reflects the elemental composition and element valence state of the sample surface; a is the full spectrum, indicating the presence and content of Fe, C, N, O, and Ho elements, where the peak intensity indicates their relative content. b, c, d, e, and f are the spectra of Fe, N, C, O, and Ho, respectively, revealing the valence states of these elements and their bonding types. The three peaks in Figure d represent the peaks of C=O (288.43 eV), CO (285.98 eV), and CC (284.78 eV) bonds, respectively, indicating the presence of MOFs. The peak in Figure f also shows that Ho 3+ Successful doping.
[0054] Figure 5 The X-ray diffraction spectrum (XRD) of the Ho-MOF-modified α-Fe2O3 photoanode catalyst (α-Fe2O3 / Ho-MOF) and the α-Fe2O3 photoanode obtained in Example 1 of the present invention; the peaks of Ho-MOF and α-Fe2O3 can be seen, indicating that the Ho-MOF-modified α-Fe2O3 photoanode catalyst was successfully prepared;
[0055] Figure 6 The infrared spectra of the Ho-MOF modified α-Fe2O3 photoanode catalyst (α-Fe2O3 / Ho-MOF) and the α-Fe2O3 photoanode obtained in Example 1 of the present invention; Figure 6 The wavelengths of 1500-1740 cm -1 The -COOH peak at 3050 cm -1 The -OH peak at 40° and 80°, proving that Ho-MOF was successfully loaded onto the α-Fe2O3 photoanode catalyst.
[0056] Figure 7 and Figure 8The LSV curves and it curves of the Ho-MOF modified α-Fe2O3 photoanode catalyst and the α-Fe2O3 photoanode catalyst in 1M NaOH solution obtained in Example 1 are shown respectively. The specific test method is: using an electrochemical workstation with a xenon lamp as the light source, 1M NaOH as the electrolyte, Ag / AgCl electrode as the reference electrode, platinum sheet as the counter electrode, and the catalyst as the working electrode, the LSV and it and other photoelectrochemical tests are performed using CHI66E software. The α-Fe2O3 photoanode is the standard catalyst (α-Fe2O3 shown in the figure). Figure 7 It can be seen that the Ho-MOF modified α-Fe2O3 photoanode catalyst prepared in Example 1 is RHE The photocurrent density under bias voltage reached 0.57 mA cm -2 , compared with pure α-Fe2O3 (photocurrent density is 0.16mAcm -2 ) is significantly improved. Figure 8 It can be seen that the Ho-MOF modified α-Fe2O3 photoanode catalyst prepared in Example 1 is RHE The photocurrent density has no obvious decay within 10 minutes under bias. The photocurrent density of α-Fe2O3 photoanode catalyst is significantly lower than that of Ho-MOF modified α-Fe2O3 photoanode catalyst, and the photocurrent density has no obvious decay within 10 minutes.
[0057] Example 2
[0058] The preparation method of the Ho-MOF modified α-Fe2O3 photoanode catalyst is different from that of Example 1 only in that: in (2), 10 mL of N,N-dimethylformamide solution (DMF) and 2.5 mL of anhydrous ethanol solution are mixed evenly; the remaining steps are the same as those of Example 1.
[0059] Characterization showed that the product obtained in this example had a heterogeneous structure and uniform morphology.
[0060] The same method as in Example 1 was used to test the prepared Ho-MOF-modified α-Fe2O3 photoanode catalyst at 1.23 V. RHE The photocurrent density under bias voltage reached 0.54 mA cm -2 , there is no obvious decay of photocurrent density within 10 minutes.
[0061] Example 3
[0062] The preparation method of the Ho-MOF modified α-Fe2O3 photoanode catalyst is different from that of Example 1 only in that: in (2), 5 mL of N,N-dimethylformamide solution (DMF) and 2.5 mL of anhydrous ethanol solution are mixed evenly; the remaining steps are the same as those of Example 1.
[0063] Characterization showed that the product obtained in this example had a heterogeneous structure and uniform morphology.
[0064] The same method as in Example 1 was used to test the prepared Ho-MOF-modified α-Fe2O3 photoanode catalyst at 1.23 V. RHE The photocurrent density under bias voltage reached 0.49 mA cm -2 , there is no obvious decay of photocurrent density within 10 minutes.
[0065] Comparative Example 1
[0066] The preparation method of the Ho-MOF modified α-Fe2O3 photoanode catalyst comprises the following steps:
[0067] 3.5 g FeCl3·6H2O and 3 g NaNO3 were dissolved in 50 ml deionized water to form a mixed aqueous solution, and 0.15 ml concentrated hydrochloric acid was added to the mixed aqueous solution, and stirred for 15 min to obtain a precursor solution; the pretreated FTO glass conductive surface was placed downward in a polytetrafluoroethylene reactor, and 10 ml of the precursor solution was added along the inner wall of the polytetrafluoroethylene reactor, and the reactor was sealed with a stainless steel hydrothermal reactor, and reacted at 100 ° C for 24 h. After the reaction was completed, it was cooled to room temperature, and the obtained product was washed and dried with a mixed solution of N, N-dimethylformamide and ethanol, and then air annealed at 500 ° C for 2 h in a tube furnace, and then treated with an ozone cleaner for 10 min to obtain an α-Fe2O3 photoanode.
[0068] Modification of Ho-MOF:
[0069] (1) Dissolve 0.95 g of HoCl3·6H2O in 15 ml of DMF solvent to form a metal salt solution;
[0070] (2) 7.5 mL of N,N-dimethylformamide solution (DMF) and 2.5 mL of anhydrous ethanol solution were mixed evenly, and then 78 mg of chiral H3L ligand was added, and the mixture was stirred and ultrasonically mixed to obtain a mixed solution;
[0071] (3) adding the metal salt solution obtained in step (1) to the mixed solution obtained in step (2), and then adding 0.1 mL of formic acid;
[0072] (4) Place the conductive surface of the α-Fe2O3 photoanode downward in a polytetrafluoroethylene reactor, and then slowly inject the solution obtained in step (3) along the non-conductive surface of the α-Fe2O3 photoanode, seal it with a stainless steel hydrothermal reactor, and react at 125°C for 14 hours to obtain Ho-MOF. The obtained product is washed three times with a mixed solution of N,N-dimethylformamide and ethanol and dried at 60°C to obtain a Ho-MOF-modified α-Fe2O3 photoanode catalyst.
[0073] Characterization showed that the product obtained in this comparative example had a heterogeneous structure and uniform morphology.
[0074] The same method as in Example 1 was used to test the Ho-MOF-modified α-Fe2O3 photoanode catalyst prepared in this comparative example at 1.23V. RHE The photocurrent density under bias voltage reached 0.32 mA cm -2 , there is no obvious decay of photocurrent density within 10 minutes.
[0075] Example 4
[0076] The preparation method of the Ho-MOF modified α-Fe2O3 photoanode catalyst comprises the following steps:
[0077] (1) 3.5 g FeCl3·6H2O and 3 g NaNO3 were dissolved in 50 ml deionized water to form a mixed aqueous solution, and 0.15 ml concentrated hydrochloric acid was added to the mixed aqueous solution, and stirred for 15 min to obtain a precursor solution; the pretreated FTO glass conductive surface was placed in a polytetrafluoroethylene reactor with the conductive surface facing downward, and 10 ml of the precursor solution was added along the inner wall of the polytetrafluoroethylene reactor, and the reactor was sealed with a stainless steel hydrothermal reactor, and reacted at 100 ° C for 24 h. After the reaction was completed, the reactor was cooled to room temperature, and the obtained product was washed and dried with a mixed solution of N, N-dimethylformamide and ethanol, and then air annealed at 500 ° C for 2 h in a tube furnace, and then treated with an ozone cleaner for 10 min to obtain an α-Fe2O3 photoanode;
[0078] Modification of Ho-MOF:
[0079] (1) Dissolve 0.95 g of HoCl3·6H2O in 15 ml of DMF solvent to form a metal salt solution;
[0080] (2) 7.5 mL of N,N-dimethylformamide solution (DMF) and 2.5 mL of anhydrous ethanol solution were mixed evenly, and then 312 mg of chiral H3L ligand was added, and the mixture was stirred and ultrasonically mixed to obtain a mixed solution;
[0081] (3) adding the metal salt solution obtained in step (1) to the mixed solution obtained in step (2), and then adding 0.1 mL of formic acid;
[0082] (4) Place the conductive surface of the α-Fe2O3 photoanode downward in a polytetrafluoroethylene reactor, and then slowly inject the solution obtained in step (3) along the non-conductive surface of the α-Fe2O3 photoanode, seal it with a stainless steel hydrothermal reactor, and react at 125°C for 14 hours to obtain Ho-MOF. The obtained product is washed three times with a mixed solution of N,N-dimethylformamide and ethanol and dried at 60°C to obtain a Ho-MOF-modified α-Fe2O3 photoanode catalyst.
[0083] Characterization showed that the product obtained in this example had a heterogeneous structure and uniform morphology.
[0084] The same method as in Example 1 was used to test the prepared Ho-MOF-modified α-Fe2O3 photoanode catalyst at 1.23 V. RHE The photocurrent density under bias voltage reaches 0.50 mA cm -2 , there is no obvious decay of photocurrent density within 10 minutes.
[0085] Comparative Example 2
[0086] The preparation method of the Ho-MOF modified α-Fe2O3 photoanode catalyst comprises the following steps:
[0087] 3.5 g of FeCl3·6H2O and 3 g of NaNO3 were dissolved in 50 ml of deionized water to form a mixed aqueous solution, and then 0.15 ml of concentrated hydrochloric acid was added to the obtained mixed aqueous solution, and stirred for 15 min to obtain a precursor solution; the pretreated FTO glass conductive surface was placed in a polytetrafluoroethylene reactor with the conductive surface facing downward, and 10 ml of the precursor solution was added along the inner wall of the polytetrafluoroethylene reactor, and the reactor was sealed with a stainless steel hydrothermal reactor, and reacted at 100 ° C for 24 h. After the reaction was completed, it was cooled to room temperature, and the obtained product was washed and dried with a mixed solution of N, N-dimethylformamide and ethanol, and then air annealed at 500 ° C for 2 h in a tube furnace, and then treated with an ozone cleaner for 10 min to obtain an α-Fe2O3 photoanode;
[0088] Modification of Ho-MOF:
[0089] (1) Dissolve 0.95 g HoCl3·6H2O in 15 ml DMF solvent to form a metal salt solution
[0090] (2) 7.5 mL of N,N-dimethylformamide solution (DMF) and 2.5 mL of anhydrous ethanol solution were mixed evenly, and then 145 mg of chiral H3L ligand was added, and the mixture was stirred and ultrasonically mixed to obtain a mixed solution;
[0091] (3) adding the metal salt solution obtained in step (1) to the mixed solution obtained in step (2), and then adding 0.5 mL of formic acid;
[0092] (4) Place the conductive surface of the α-Fe2O3 photoanode facing downward in a polytetrafluoroethylene reactor, and then slowly inject the solution obtained in step (3) along the non-conductive surface of the α-Fe2O3 photoanode, seal it with a stainless steel hydrothermal reactor, and react at 125°C for 14 hours to obtain Ho-MOF. The obtained product is washed three times with a mixed solution of N,N-dimethylformamide and ethanol, and dried at 60°C to obtain a Ho-MOF-modified α-Fe2O3 photoanode catalyst;
[0093] Characterization showed that the product obtained in this comparative example had a heterogeneous structure and uniform morphology.
[0094] The same method as in Example 1 was used to test the Ho-MOF-modified α-Fe2O3 photoanode catalyst prepared in this comparative example at 1.23V. RHE The photocurrent density under bias voltage reached 0.31 mA cm -2 , there is no obvious decay of photocurrent density within 10 minutes.
[0095] Example 5
[0096] The preparation method of the Ho-MOF modified α-Fe2O3 photoanode catalyst comprises the following steps:
[0097] 3.5 g FeCl3·6H2O and 3 g NaNO3 were dissolved in 50 ml deionized water to form a mixed aqueous solution, and 0.15 ml concentrated hydrochloric acid was added to the obtained mixed aqueous solution and stirred for 15 min to obtain a precursor solution; the pretreated FTO glass conductive surface was placed downward in a polytetrafluoroethylene reactor, and 10 ml of the precursor solution was added along the inner wall of the polytetrafluoroethylene reactor, and the reactor was sealed with a stainless steel hydrothermal reactor, and reacted at 100 ° C for 24 h. After the reaction was completed, it was cooled to room temperature, and the obtained product was washed and dried with a mixed solution of N, N-dimethylformamide and ethanol, and then air annealed at 500 ° C for 2 h in a tube furnace, and then treated with an ozone cleaner for 10 min to obtain an α-Fe2O3 photoanode.
[0098] Modification of Ho-MOF:
[0099] (1) Dissolve 0.95 g of HoCl3·6H2O in 15 ml of DMF solvent to form a metal salt solution;
[0100] (2) 7.5 mL of N,N-dimethylformamide solution (DMF) and 2.5 mL of anhydrous ethanol solution were mixed evenly, and then 156 mg of chiral H3L ligand was added, and the mixture was stirred and ultrasonically mixed to obtain a mixed solution;
[0101] (3) adding the metal salt solution obtained in step (1) to the mixed solution obtained in step (2), and then adding 0.05 mL of formic acid;
[0102] (4) Place the conductive surface of the α-Fe2O3 photoanode facing downward in a polytetrafluoroethylene reactor, and then slowly inject the solution obtained in step (3) along the non-conductive surface of the α-Fe2O3 photoanode, seal it with a stainless steel hydrothermal reactor, and react at 125°C for 14 hours to obtain Ho-MOF. The obtained product is washed three times with a mixed solution of N,N-dimethylformamide and ethanol, and dried at 60°C to obtain a Ho-MOF-modified α-Fe2O3 photoanode catalyst;
[0103] Characterization showed that the product obtained in this example had a heterogeneous structure and uniform morphology.
[0104] The same method as in Example 1 was used to test the prepared Ho-MOF-modified α-Fe2O3 photoanode catalyst at 1.23 V. RHE The photocurrent density under bias voltage reached 0.51 mA cm -2 , there is no obvious decay of photocurrent density within 10 minutes.
[0105] Example 6
[0106] A method for preparing a Ho-MOF modified α-Fe2O3 photoanode catalyst, wherein the steps thereof are different from those of Example 1 only in that the reaction temperature of (4) in the Ho-MOF modification is 140° C. The remaining steps are the same as those of Example 1.
[0107] Characterization showed that the product obtained in this example had a heterogeneous structure and uniform morphology.
[0108] The same method as in Example 1 was used to test the prepared Ho-MOF-modified α-Fe2O3 photoanode catalyst at 1.23 V. RHE The photocurrent density under bias voltage reached 0.53 mA cm -2 , there is no obvious decay of photocurrent density within 10 minutes.
[0109] Example 7
[0110] A method for preparing a Ho-MOF modified α-Fe2O3 photoanode catalyst, wherein the steps thereof are different from those of Example 1 only in that the reaction temperature of (4) in the Ho-MOF modification is 110°C.
[0111] Characterization showed that the product obtained in this example had a heterogeneous structure and uniform morphology.
[0112] The same method as in Example 1 was used to test the prepared Ho-MOF-modified α-Fe2O3 photoanode catalyst at 1.23 V.RHE The photocurrent density under bias voltage reached 0.52 mA cm -2 , there is no obvious decay of photocurrent density within 10 minutes.
[0113] Example 8
[0114] A method for preparing a Ho-MOF modified α-Fe2O3 photoanode catalyst, wherein the steps thereof are different from those of Example 1 only in that the reaction time of (4) in the Ho-MOF modification is 16 h.
[0115] Characterization showed that the product obtained in this example had a heterogeneous structure and uniform morphology.
[0116] The same method as in Example 1 was used to test the prepared Ho-MOF-modified α-Fe2O3 photoanode catalyst at 1.23 V. RHE The photocurrent density under bias voltage reached 0.54 mA cm -2 , there is no obvious decay of photocurrent density within 10 minutes.
[0117] Example 9
[0118] A method for preparing a Ho-MOF modified α-Fe2O3 photoanode catalyst, wherein the steps thereof are different from those of Example 1 only in that the reaction time of (4) in the Ho-MOF modification is 12 h.
[0119] Characterization showed that the product obtained in this example had a heterogeneous structure and uniform morphology.
[0120] The same method as in Example 1 was used to test the prepared Ho-MOF-modified α-Fe2O3 photoanode catalyst at 1.23 V. RHE The photocurrent density under bias voltage reached 0.47 mA cm -2 , there is no obvious decay of photocurrent density within 10 minutes.
[0121] Comparative Example 3
[0122] A method for preparing a La-MOF-modified α-Fe2O3 photoanode catalyst, wherein the steps thereof are different from those of Example 1 only in that LaCl3·6H2O is used instead of HoCl3·6H2O for modification.
[0123] After characterization, the product obtained in this comparative example cannot present a heterogeneous structure, such as Fig.11 shown.
[0124] The La-MOF-modified α-Fe2O3 photoanode catalyst prepared in this comparative example was tested in the same manner as in Example 1 at 1.23 V. RHEThe photocurrent density under bias voltage reached 0.26 mA cm -2 , there is no obvious decay of photocurrent density within 10 minutes.
[0125] Depend on Fig. 9 It can be seen that the La-MOF modified α-Fe2O3 photoanode catalyst prepared in this comparative example 3 has a RHE The photocurrent density under bias voltage reached 0.26 mA cm -2 , the photocurrent density of the α-Fe2O3 photoanode catalyst modified by Ho-MOF in Example 1 is lower.
[0126] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a Ho-MOF modified α-Fe2O3 photoanode catalyst, characterized in that: The following steps are involved: S1. Generate β-FeOOH on FTO conductive glass to obtain FTO / β-FeOOH photoelectrode; anneal the FTO / β-FeOOH photoelectrode in air atmosphere to obtain FTO / α-Fe2O3 photoanode; S2, formic acid, N, N-dimethylformamide, ethanol, chiral H3L ligand and holmium salt are mixed uniformly to form a precursor solution; wherein the chiral H3L ligand has a structural formula of The mass ratio of the holmium salt to the chiral H3L ligand is 0.95 g:156-350 mg; S3. Place the FTO / α-Fe2O3 photoanode and the precursor solution in a hydrothermal reaction device, seal it and react it, and cool it after the reaction to obtain the Ho-MOF modified α-Fe2O3 photoanode catalyst.
2. The method for preparing the Ho-MOF modified α-Fe2O3 photoanode catalyst according to claim 1, characterized in that: In S1, the annealing temperature is 500° C. and the time is 2 h.
3. The method for preparing the Ho-MOF modified α-Fe2O3 photoanode catalyst according to claim 1, characterized in that: In S2, the volume ratio of ethanol to N,N-dimethylformamide is 2.5:8-25.
4. The method for preparing the Ho-MOF modified α-Fe2O3 photoanode catalyst according to claim 1, characterized in that: In S2, the mass volume ratio of the chiral H3L ligand to ethanol is 156-350 mg:2.5 ml.
5. The method for preparing the Ho-MOF modified α-Fe2O3 photoanode catalyst according to claim 1, characterized in that: In S2, the ratio of the holmium salt to the chiral H3L ligand is 0.95 g:156-312 mg.
6. The method for preparing the Ho-MOF modified α-Fe2O3 photoanode catalyst according to claim 1, characterized in that: In S2, the concentration of the chiral H3L ligand in the precursor solution is 5.5-39 mg / ml.
7. The method for preparing the Ho-MOF modified α-Fe2O3 photoanode catalyst according to claim 1, characterized in that: In S3, the reaction temperature is 110-140°C and the reaction time is 12-16 hours.
8. The method for preparing the Ho-MOF modified α-Fe2O3 photoanode catalyst according to any one of claims 1 to 7, characterized in that: In S1, the following steps are specifically included: mixing ferric chloride, sodium nitrate, concentrated hydrochloric acid and water to form a mixed solution; transferring the mixed solution and FTO conductive glass to a hydrothermal reaction device, sealing and reacting; cooling to room temperature after the reaction is completed, and washing, drying and annealing the obtained product in an air atmosphere to obtain the FTO / α-Fe2O3 photoanode.
9. A Ho-MOF modified α-Fe2O3 photoanode catalyst, characterized in that: The photoanode catalyst is prepared by the method for preparing a Ho-MOF-modified α-Fe2O3 photoanode catalyst as described in any one of claims 1 to 8.
10. Use of the Ho-MOF modified α-Fe2O3 photoanode catalyst as claimed in claim 9 as a photoelectrocatalyst for catalyzing water oxidation reaction.
Citation Information
Patent Citations
Preparation method and application of transition / rare earth multi-metal co-doped phosphide
CN113832494A
Co < 2 + >-doped CdMOFs-cadmium sulfide photo-anode catalyst as well as preparation method and application thereof