Method for eliminating generation of small-angle grain boundary defects in tellurium dioxide single crystal growth

By using the 'commutation' growth method and crucible drop method in the growth of tellurium dioxide single crystals, combined with solid-liquid interface control and temperature compensation, the problem of difficult to eliminate small-angle grain boundary defects is solved, and the yield and crystal rod utilization are improved rate, reduces cost and quality fluctuations.

CN118910731AActive Publication Date: 2024-11-08XIAMEN SENYI QUANTUM MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410943738.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-08
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

In the prior art, small angle grain boundary defects in the growth of single crystals of tellurium dioxide are difficult to completely eliminate, resulting in fluctuations in yield and low utilization rate of crystal rods. Especially when there are small angle grain boundaries inside the seed crystal, the existing iterative method is costly. And inefficient.

Method used

Using the 'commutation' growth method, seed crystal processing is performed by using the (1-10) plane as the long crystal plane, vertically or parallel to the [110] crystal direction, and the temperature gradient and descent rate of the solid-liquid interface are controlled in the crucible descent method. , combined with system temperature compensation and in-situ annealing treatment, eliminate small-angle grain boundary defects.

Benefits of technology

By reversing growth instead of multiple iterations, the yield rate is significantly improved, quality fluctuations are reduced, and the overall utilization rate of crystal rods is improved, reducing costs and processing losses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910731A_ABST
    Figure CN118910731A_ABST
Patent Text Reader

Abstract

The invention discloses a method for eliminating generation of small-angle grain boundary defects in tellurium dioxide single crystal growth. The method comprises the steps of seed crystal processing, seed crystal reversing treatment and tellurium dioxide single crystal growth through a Bridgman-Stockbarger method. Wherein the reversing treatment operation of the seed crystal refers to that a (1-10) crystal face is used as a long crystal face instead of a traditional (110) crystal face. According to the method, seed crystal reversing treatment is adopted for growing the single crystal, the mode of eliminating defects through multiple iterations is replaced, the overall utilization rate of a crystal bar and the quality of the seed crystal are improved, and therefore the yield of the TeO2 single crystal is further improved, and quality fluctuation is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of artificial crystal growth equipment, and in particular to a method for eliminating small-angle grain boundary defects in the growth of tellurium dioxide single crystals. Background Art

[0002] Tellurium dioxide (TeO2) crystal is an acousto-optic material with excellent acousto-optic properties and is widely used in pulse fiber laser modulation and lidar. In the existing industrial growth technology, there are two conventional methods for growing TeO2 single crystals: the Czochralski method and the crucible descent method. The Czochralski method eliminates most of the dislocation defects and small-angle grain boundaries in the seed crystal by necking and shouldering the seed crystal to grow high-quality TeO2 single crystals. The crucible descent method is quite different from the Czochralski method in that it cannot eliminate dislocations and defects by effectively necking. In addition, the crucible descent method is prone to dislocation proliferation and aggregation into small-angle grain boundaries during the shouldering growth process. Generally, a small-angle grain boundary refers to a grain boundary between adjacent grains with a phase difference of less than 10°.

[0003] In the prior art, high-quality TeO2 single crystals are usually grown using equal-diameter seed crystals. There are two options for high-quality equal-diameter seed crystals: 1. Select the defect-free part of the entire crystal (product grade) for crystal growth; 2. Select the slightly defective part for iteration to eliminate the defects. The cost of these two options is relatively high. In addition, the multiple iteration method is also prone to fluctuations in yield, because multiple iterative growth can gradually eliminate the small-angle grain boundaries near the outer layer, while the small-angle grain boundaries in the middle are difficult to completely eliminate.

[0004] In order to solve the above problems, the present invention provides a method for growing high-quality TeO2 single crystals when there are small-angle grain boundaries inside the seed crystal. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, one of the objects of the present invention is to provide a method for eliminating the generation of small-angle grain boundary defects in the growth of tellurium dioxide single crystals, thereby improving the quality of seed crystals and the utilization rate of crystal rods. In particular, when small-angle grain boundaries exist inside the crystal rods, a "reversing" growth method is adopted to completely eliminate the defects, replacing the multiple iteration methods in the prior art, thereby improving the overall utilization rate of the crystal rods and the quality of seed crystals, thereby further improving the yield of TeO2 single crystals and reducing quality fluctuations.

[0006] A method for eliminating small-angle grain boundary defects in the growth of tellurium dioxide single crystals comprises the following steps:

[0007] A. Processing of seed crystals: cutting the crystal rod into crystal blocks, controlling the crystal orientation deviation of the crystal blocks within 0.5°, and then rough grinding, fine grinding, and polishing; at the same time, controlling the temperature of the cutting fluid, grinding fluid, and polishing fluid during the rough grinding, fine grinding, and polishing process, and using an infrared thermometer to regularly measure the temperature difference between the inside and outside of the seed crystal; after polishing, the required seed crystals are obtained, and the internal quality screening is performed in a dark room using a laser, and the distribution position and quantity of the corresponding small-angle grain boundaries are marked on the seed crystals with a marker pen;

[0008] B. The seed crystal is subjected to a reversing operation, that is, the (1-10) plane is used as the growth plane, and the internal small-angle grain boundary is perpendicular to the [1-10] crystal direction or parallel to the

[110] crystal direction;

[0009] C. placing the obtained seed crystal into a crucible with the growth surface facing upward, placing the tellurium dioxide raw material on top of the seed crystal, and sealing the crucible, and then placing it in a crystal growth furnace, heating and melting the tellurium dioxide raw material and the top of the seed crystal to achieve seeding growth;

[0010] D. growing a tellurium dioxide single crystal by a crucible descent method, controlling the temperature gradient of the solid-liquid interface and the descent rate of the crucible; after the growth stage is stable, using a system temperature compensation method to reduce the acceleration during the crystal growth process; and performing an in-situ annealing treatment to obtain the tellurium dioxide single crystal.

[0011] Furthermore, the number of small-angle grain boundaries inside the seed crystal does not exceed 3, and the cross-sectional dimension is 0.5-1 mm smaller than the cross-sectional dimension of the crucible, the chamfer dimensions of the four sides are R2-R3, and the height is above 30 mm.

[0012] Furthermore, the long crystal face is the end face with fewer defects on the (1-10) face, the face with more defects is marked as the bottom face, and the small-angle grain boundary is within 15 mm from the long crystal face.

[0013] Furthermore, the crystal orientation of the (110) plane of the seed crystal is 13°06′±30′, the crystal orientation of the (001) plane is 23°53′±30′, and the crystal orientation of the (1-10) plane is 13°06′±30′.

[0014] Furthermore, in step A, the temperature difference between the inside of the seed crystal and the outside is no more than 5°C.

[0015] Preferably, the seed crystals in step A are moved into a beaker containing 95% anhydrous ethanol and ultrasonically cleaned for 20 minutes. After cleaning, the seed crystals are placed on a pad to dry, marked and set aside.

[0016] Furthermore, the crystal orientation deviation control in step A adopts a combination of an orientation instrument and manual fine grinding to grind the surface with a large orientation angle in steps, and gradually control the crystal orientation deviation within 0.5°.

[0017] Preferably, the specific process of step A polishing is: using W360 silicon carbide sand on a single-axis table, using 80-100rpm to level each plane, so that the crystal orientation angle of the crystal block is within 1° and there is no step on the surface; chamfering each edge of the crystal block (R2-R3) for protection; using W10 fine silicon carbide sand on a single-axis table, using 80-100rpm to finely grind the surface roughness within PV0.01, the crystal orientation angle within 0.5 degrees, and the dimensional tolerance is ±0.01mm; then using cerium oxide polishing liquid at a speed of 80-120rpm to polish, so that the surface roughness reaches within PV0.001, and the optical index is 40-20.

[0018] Preferably, the temperature gradient of the solid-liquid interface in step D is set within the range of 20 to 50° C. / cm, and the descent rate of the crucible is controlled between 0.1 and 1.0 mm / h.

[0019] Beneficial effects: 1. Replacing multiple iterations with a reversing growth method can further improve the yield rate and reduce quality fluctuations;

[0020] Second, the processing allowance and utilization rate of the square crystal rod are significantly related to the crystal orientation deviation of the seed crystal. The present invention controls the crystal orientation deviation during the seed crystal processing within 0.5 degrees, effectively improving the overall utilization rate of the crystal rod. In the prior art, the crystal orientation deviation of the square seed crystal processing is usually controlled within 2 degrees, and the processing loss is large.

[0021] 3. Solve the cleavage problem caused by temperature difference during the processing of TeO2 seed crystals by regular temperature measurement and temperature control, and further improve the quality of seed crystals. High-quality TeO2 single crystal growth reversal technology, anti-cleavage technology during TeO2 seed crystal processing. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a schematic diagram of the processing of square TeO2 seed crystals.

[0023] Figure 2 This is a schematic diagram of the seed crystal after processing. The reversal treatment uses the (1-10) plane as the crystal growth plane.

[0024] Figure 3 This is a photo of the surface morphology of the seed crystal before processing.

[0025] Figure 4 This is the situation of the seed crystal in the dark room after reversal growth.

[0026] Explanation of reference numerals: 1, crystal rod; 10, seed crystal; 20, low-angle grain boundary; 30, (110) plane; 40, (1-10) plane; 50, padding DETAILED DESCRIPTION

[0027] In order to better understand the technical solution of the present invention, the following is a detailed description in conjunction with specific embodiments. It should be clear that the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] The acquisition of high-quality TeO2 single crystals is closely related to the quality of the seed crystal. When there are slight defects in the seed crystal or defects generated during the processing, on the other hand, the single crystal grown by the crucible descent method is prone to dislocation proliferation during the shoulder growth process, and defects such as aggregation into small-angle grain boundaries will affect the production efficiency of tellurium dioxide single crystals.

[0029] TeO2 crystal is a typical tetragonal crystal, in which the (110) face 30 is a light-transmitting face, which is usually the main growth direction of the crystal, and the orientation accuracy is required to be controlled at 13°06'±30', while the (001) face is a bonding face with the LN crystal, and the orientation accuracy is required to be controlled at 23°53'±30'. The other face is the (1-10) face 40. Due to the special physical properties of the tetragonal crystal system, the (110) face 30 and the (1-10) face 40 are equivalent faces, and theoretically, the directions can be interchanged, and the equivalent reversing growth of the crystal can be achieved on the (1-10) face 40. This is also the source of the technical concept of the present invention.

[0030] The existing process generally uses the (110) plane 30 as the growth plane of the seed crystal 10. When there are defects in the seed crystal 10, the slightly defective part is selected for iteration to eliminate the defects. For example, the small angle grain boundary 20 on the outer layer of the seed crystal 10 can be gradually eliminated through multiple iterations of growth, but the small angle grain boundary 20 in the middle is difficult to be completely eliminated. If such a seed crystal 10 is used to inoculate the growth of tellurium dioxide single crystals, the small angle grain boundary 20 will be inherited to the new crystal, so the industry will not select the crystal rod 1 with a small angle grain boundary 20 in the middle as the seed crystal 10.

[0031] In this regard, the present invention provides a method for eliminating the generation of small-angle grain boundary defects in the growth of tellurium dioxide single crystals, comprising the following steps:

[0032] A. Processing of the seed crystal 10: cutting the crystal rod 1 into crystal blocks, selecting a suitable crystal block, controlling its crystal orientation deviation within 0.5 degrees, and performing rough grinding, fine grinding, and polishing; at the same time, controlling the temperature of the cutting liquid, grinding liquid, and polishing liquid during the rough grinding, fine grinding, and polishing process, and using an infrared thermometer to regularly measure the temperature difference between the inside and the outside of the seed crystal 10; after polishing, the desired seed crystal 10 is obtained, and internal quality screening is performed in a dark room using a laser, and the distribution position and quantity of the corresponding low-angle grain boundaries 20 are marked on the seed crystal 10 using a marker.

[0033] B. The seed crystal 10 is subjected to a reversing operation, that is, the (1-10) plane 40 is used as the growth plane, and the internal low-angle grain boundary 20 is perpendicular or nearly perpendicular to the [1-10] crystal direction or parallel to the

[110] crystal direction.

[0034] C. Load the obtained seed crystal 10 into a crucible with the growth surface facing upward, place the tellurium dioxide raw material above the seed crystal 10, and seal the crucible. Then put it into a crystal growth furnace, heat and melt the tellurium dioxide raw material and the top of the seed crystal 10 to achieve seeding growth.

[0035] D. growing a tellurium dioxide single crystal by a crucible descent method, controlling the temperature gradient of the solid-liquid interface and the descent rate of the crucible; after the growth stage is stable, using a system temperature compensation method to reduce the acceleration during the crystal growth process; and performing an in-situ annealing treatment to obtain the tellurium dioxide single crystal.

[0036] Among them, the selection principles of the crystal block as the seed crystal 10 are as follows: 1. The crystal block is required to have no internal cracks and cloud layers on a macro scale; 2. The number of small-angle grain boundaries 20 is ≤3; 3. The cross-sectional size is controlled to be 0.5-1mm smaller than the crucible cross-sectional size, the four-sided chamfer size is R2-R3, and the height is controlled to be above 30mm.

[0037] The more specific steps of processing the seed crystal 10 are to use a conventional

[110] oriented crystal rod to cut into the required size of the seed crystal 10 blank, grind the three groups of directions of length, width and height to the specified size and crystal orientation range respectively, and then perform a rough grinding process. After the rough grinding, enter the fine grinding process. After the fine grinding is completed, add a certain particle size of cerium oxide polishing powder on the polishing machine to perform four-sided detection polishing, including two sides of the (1-10) face 40 and two sides of the (001) face. During the grinding and polishing process, the temperature difference between the crystal block and the external environment temperature must be controlled, and the requirement is ≤5°C to avoid

[010] direction cleavage caused by the ambient temperature difference inside and outside the crystal block. If the temperature difference exceeds 5°C, the crystal block needs to be left still for a period of time, and the processing can continue after the internal and external temperatures of the crystal are stable and balanced.

[0038] Preferably, after the seed crystal 10 is processed, in order to eliminate the pollution caused by the organic materials and metal grinding disc used in the processing steps, the seed crystal 10 is ultrasonically cleaned for 20 minutes, wherein the solution used to soak the seed crystal 10 during the ultrasonic treatment is a 95% anhydrous ethanol solution, thereby further improving the internal quality of the crystal growth.

[0039] Furthermore, the end face of the (1-10) plane 40 with fewer defects is marked as the long crystal face, and the end face with more defects is marked as the bottom face, and the small-angle grain boundary is within 15 mm from the long crystal face.

[0040] It should be noted that when using the (1-10) plane 40 as the crystal growth plane, the selection and processing of the seed crystal 10 is one of the key steps, because tellurium dioxide is a covalent bond crystal, slightly soluble in water, and will decompose when encountering strong acids and alkalis. It has low hardness and is relatively soft, and is easily scratched during polishing; its thermal conductivity is also low, and it is easy to crack during processing. On the other hand, the processing allowance and utilization rate of the square crystal rod are significantly correlated with the crystal orientation deviation of the seed crystal 10. As shown in Table 1, the present invention can control the crystal orientation deviation within 0.5 degrees, greatly improving the utilization rate of the crystal rod. In the prior art, the crystal orientation deviation of the square seed crystal processing is usually controlled within 2 degrees, and the processing loss is relatively large.

[0041] Another key factor in using the (1-10) plane 40 as the crystal growth plane is to control the seeding growth of the seed crystal 10, especially to control the growth at the solid-liquid interface. No small-angle grain boundaries 20 or other defects can exist near the solid-liquid interface.

[0042] Example: The specific implementation method is as follows. Taking the processing of 35*25*50-55mm square high-quality TeO2 seed crystal 10 as an example, several 35*25*200mm B-type

[110] direction growing crystal rods 1 are selected. The B-type crystal rod 1 refers to a crystal rod with 1-3 internal low-angle grain boundaries 20. Figure 1 As shown, the crystal rod 1 is processed in sections, and each can be cut into 5-6 crystal blocks of 35*25*36mm. After cutting, the size and direction of the crystal blocks are roughly ground, finely ground, and polished. In the process of cutting, grinding and polishing, the temperature of the cutting liquid, grinding liquid and polishing liquid is strictly controlled. An infrared handheld thermometer is used to regularly measure the temperature difference between the inside and outside of the seed crystal 10 and control it at 2-5°C. For example, the mixing ratio of hot water and cold water can be controlled by a water heater to achieve relatively accurate temperature control.

[0043] The specific process of grinding and polishing: Use W360 silicon carbide sand on a single-axis table, use 80-100rpm to level each plane, so that the crystal orientation angle of the crystal block is within 1° and there is no step on the surface. Chamfer each edge of the crystal block (R2-R3) for protection. Use W10 fine silicon carbide sand on a single-axis table, use 80-100rpm to finely grind the surface roughness within PV0.01, the crystal orientation angle within 0.5 degrees, and the dimensional tolerance is ±0.01mm. Then use cerium oxide polishing liquid at a speed of 80-120rpm to polish, so that the surface roughness reaches within PV0.001, and the optical index is 40-20.

[0044] According to the principle of seed crystal 10 selection, after polishing, a 400mW 532nm laser is used to perform internal quality screening in a dark room, and a marker is used to mark the distribution position and number of the corresponding low-angle grain boundaries 20 on the polished crystal block. After the selection is completed, the reversing processing operation is performed, such as Figures 1 to 3 As shown, Figure 2 It is a schematic diagram of the crystal plane of the seed crystal 10. The reversal process is to use the (1-10) plane 40 as the crystal growth plane instead of the (110) plane 30. Figure 3 The image shows the morphology of the processed seed crystal (110) surface, where the low-angle grain boundary 20 can be clearly seen. The end face of the (1-10) surface 40 with fewer defects is marked as the T face (i.e., the long crystal face), and the end face with more defects is marked as the B face (i.e., the bottom face). After the seed crystal 10 reversing step is completed, it is moved into a large beaker filled with 95% anhydrous ethanol and ultrasonically cleaned in an ultrasonic machine for 20 minutes. After the cleaning is completed, the seed crystal 10 and the pad are combined and dried. After the treatment is completed, the corresponding markings and distinctions are made and transferred to a moisture-proof cabinet for standby use.

[0045] Comparative example: Taking the processing of 35*25*50-55mm seed crystal 10 as an example, several 35*25*200mm Class B

[110] direction grown crystal rods 1 are selected for segmented processing. Each of them can be cut into 3-4 35*25*55mm blocks. After cutting, the size and direction of the seed crystal 10 blocks are coarsely ground, finely ground and polished. The small-angle grain boundaries 20 near the edge of the crystal rod 1 that does not change direction along the

[110] growth direction gradually terminate at the outer surface of the crystal rod during the growth process. It takes 2-3 rounds of iterative growth to gradually eliminate the small-angle grain boundaries 20 near the outer layer, and it is difficult to completely eliminate the small-angle grain boundaries 20 in the middle.

[0046] Table 1 Utilization rate of

[110] orientation of crystal ingot with different orientation deviation angles

[0047]

[0048] The seed crystals 10 prepared in the embodiment and the comparative example are placed on the pads 50 in the crucible, respectively, and single crystal growth is prepared according to the process parameters of the crucible descent method. The specific steps are to load the obtained seed crystal 10 into the crucible with the growth surface facing up, place the tellurium dioxide raw material above the seed crystal 10, and seal the crucible, then put it into the crystal growth furnace, heat and melt the tellurium dioxide raw material and the top of the seed crystal 10 to achieve inoculation growth; control the temperature gradient of the solid-liquid interface and the descent rate of the crucible; after the growth stage is stable, use the system temperature compensation method to reduce the acceleration during the crystal growth process; in-situ annealing treatment to obtain the tellurium dioxide single crystal. Preferably, the temperature gradient of the solid-liquid interface is set in the range of 20 to 50°C / cm, and the crucible descent rate is controlled between 0.1 and 1.0 mm / h.

[0049] Figure 3 The morphology of the seed crystal after processing is shown, and the existence of the small-angle grain boundary 20 can be clearly seen. Figure 4This is the situation of the seed crystal 10 after the reversal growth in the dark room, using a 400mW 532nm laser. Where the small-angle grain boundary 20 exists, there will be a bright line area inside the optical path due to the refraction of light, and the uniformity of the optical path will be different. Figure 4 It can be seen that there are not so many small-angle grain boundaries 20, and the refraction of light is not very obvious.

[0050] The above description is only a preferred embodiment of the present invention and does not limit the technical scope of the present invention. Therefore, any slight modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention still fall within the protection scope of the present invention.

Claims

1. A method for eliminating small-angle grain boundary defects in the growth of tellurium dioxide single crystals, It is characterized in that The following steps are involved: A. Processing of seed crystal: cutting the crystal rod into crystal blocks, controlling the crystal orientation deviation of the crystal blocks within 0.5°, and then rough grinding, fine grinding and polishing; at the same time, controlling the temperature of the cutting liquid, grinding liquid and polishing liquid during the rough grinding, fine grinding and polishing process, and using an infrared thermometer to regularly measure the temperature difference between the inside and outside of the seed crystal; After polishing, the desired seed crystal is obtained, and internal quality screening is performed in a dark room using a laser, and the distribution position and quantity of the corresponding small-angle grain boundaries are marked on the seed crystal using a marker pen; B. The seed crystal is subjected to a reversing operation, that is, the (1-10) plane is used as the growth plane, and the internal small-angle grain boundary is perpendicular to the [1-10] crystal direction or parallel to the [110] crystal direction; C. placing the obtained seed crystal into a crucible with the growth surface facing upward, placing the tellurium dioxide raw material on top of the seed crystal, and sealing the crucible, and then placing it in a crystal growth furnace, heating and melting the tellurium dioxide raw material and the top of the seed crystal to achieve seeding growth; D. growing a tellurium dioxide single crystal by a crucible descent method, controlling the temperature gradient of the solid-liquid interface and the descent rate of the crucible; after the growth stage is stable, using a system temperature compensation method to reduce the acceleration during the crystal growth process; and performing an in-situ annealing treatment to obtain the tellurium dioxide single crystal.

2. A method for eliminating small-angle grain boundary defects in the growth of tellurium dioxide single crystals according to claim 1, It is characterized in that The number of small-angle grain boundaries inside the seed crystal does not exceed 3, and the cross-sectional dimension is 0.5-1 mm smaller than the cross-sectional dimension of the crucible, the chamfer dimensions of the four sides are R2-R3, and the height is above 30 mm.

3. A method for eliminating small-angle grain boundary defects in the growth of tellurium dioxide single crystals according to claim 1, It is characterized in that The long crystal face is the end face with fewer defects on the (1-10) face, the face with more defects is marked as the bottom face, and the small-angle grain boundary is within 15 mm from the long crystal face.

4. A method for eliminating small-angle grain boundary defects in the growth of tellurium dioxide single crystals according to claim 1, It is characterized in that The crystal orientation of the (110) plane of the seed crystal is 13°06′±30′, the crystal orientation of the (001) plane is 23°53′±30′, and the crystal orientation of the (1-10) plane is 13°06′±30′.

5. A method for eliminating small-angle grain boundary defects in the growth of tellurium dioxide single crystals according to claim 1, It is characterized in that In step A, the temperature difference between the inside of the seed crystal and the outside is no more than 5°C.

6. A method for eliminating small-angle grain boundary defects in the growth of tellurium dioxide single crystals according to claim 1, It is characterized in that The seed crystals in step A are moved into a beaker containing 95% anhydrous ethanol and ultrasonically cleaned for 20 minutes. After cleaning, the seed crystals are placed on a pad to dry, marked and set aside.

7. A method for eliminating small-angle grain boundary defects in the growth of tellurium dioxide single crystals according to claim 1, It is characterized in that In step A, the crystal orientation deviation is controlled by combining an orientation instrument with manual fine grinding, and the surface with a large orientation angle is ground step by step to gradually control the crystal orientation deviation within 0.5°.

8. A method for eliminating small-angle grain boundary defects in the growth of tellurium dioxide single crystals according to claim 4, It is characterized in that The specific process of step A polishing is as follows: using W360 silicon carbide sand on a single-axis table at 80-100 rpm to level each plane, so that the crystal orientation angle of the crystal block is within 1° and there is no step on the surface; each edge of the crystal block is chamfered (R2-R3) for protection; using W10 fine silicon carbide sand on a single-axis table at 80-100 rpm to finely grind the surface roughness within PV0.01, the crystal orientation angle within 0.5 degrees, and the dimensional tolerance is ±0.01 mm; then using cerium oxide polishing liquid at a rotation speed of 80-120 rpm to polish the surface roughness to within PV0.001, and the optical index is 40-20.

9. A method for eliminating small-angle grain boundary defects in the growth of tellurium dioxide single crystals according to claim 4, It is characterized in that In step D, the temperature gradient of the solid-liquid interface is set in the range of 20 to 50° C. / cm, and the descent rate of the crucible is controlled between 0.1 and 1.0 mm / h.

Citation Information

Patent Citations

  • Method for growing tellurium dioxide single crystal

    CN106757305A

  • Crucible lowering growth technology of Teo2 monocrystal

    CN1487126A

  • Method for cutting single crystal of tellurium dioxide

    JP1983055399A