Glass fiber cloth with low dielectric property
Through the acid leaching treatment of nanosilicate-based glass fiber yarn, the localization and cost problems of low-dielectric performance glass fiber cloth are solved, and the production of glass fiber cloth with low dielectric constant is achieved, which meets the introduction of high-speed CCL and PCB Electrical performance requirements replace imported products.
Patent Information
- Application Number
- CN202411158361.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-08
AI Technical Summary
The existing technology is difficult to produce low-dielectric glass fiber cloth in China, resulting in localization and cost problems and cannot meet the rapidly growing market demand.
Nanosilicate-based glass fiber yarn is woven, and the acid leaching is performed after the weaving is carried out to remove Na2O to form a glass fiber cloth with low dielectric constant. Through continuous drawing, weaving, acid leaching, heat cleaning and baking Dry and high temperature sintering process is realized.
The production of low-dielectric fiberglass fabrics through existing mature processes reduces costs, overcomes the complexity and technical threshold of the ternary system process, replaces imported products, and meets the dielectric performance requirements of high-speed CCL and PCB.
Smart Images

Figure CN118910782A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to glass fiber, in particular to a glass fiber cloth with low dielectric properties. Background Art
[0002] Glass fiber is an inorganic non-metallic material with excellent performance and a wide variety of types. Its advantages are good insulation, strong heat resistance, good corrosion resistance, and high mechanical strength. It is usually used as a reinforcing material in composite materials, electrical insulation materials and thermal insulation materials, circuit substrates and other industries.
[0003] Printed circuit board, abbreviated as PCB, is the key electronic interconnection component of electronic products and is known as the "mother of electronic products". With the rapid development of science and technology, the printed circuit boards used in electronic products are gradually developing towards high density, multi-layer and integration, which puts forward higher requirements on the dielectric properties of the circuit board substrate.
[0004] Copper clad laminate (CCL) is the core substrate material in PCB manufacturing. The performance, quality, processability, manufacturing level, manufacturing cost, and long-term reliability and stability of PCB depend largely on CCL. At present, the CCL industry is developing in the direction of high frequency and high speed, which has a high technical threshold. The core requirement of CCL is low dielectric. According to the size of CCL's own dielectric loss (Df) and dielectric constant (Dk), CCL can be divided into high-speed CCL and high-frequency CCL.
[0005] Low dielectric glass fiber materials are widely used as reinforcing materials in CCL and PCB. Among them, the production process of low dielectric glass fiber cloth is quite complicated. In order to reduce dielectric loss, it is generally necessary to select glass fibers with low dielectric constant or low loss factor, and use weaving, post-processing and micro-impurity control technologies to obtain basic reinforcing materials for the production of copper clad laminates and printed circuit boards. Its performance largely determines the electrical properties, mechanical properties, dimensional stability and other important properties of CCL and PCB. Due to the high technical threshold, low dielectric glass fiber cloth is currently mainly imported products. Due to trade and production capacity restrictions, it cannot meet the growing domestic market demand. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a glass fiber cloth with low dielectric properties which can replace imported products to achieve localization and reduce costs.
[0007] To solve the above technical problems, the technical solution of the present invention is: a low dielectric glass fiber cloth, the innovation of which is: the low dielectric glass fiber cloth is woven from glass fiber yarn, the glass fiber yarn is nanosilicate glass fiber, and is acid leached after weaving.
[0008] Preferably, the low dielectric glass fiber cloth comprises at least the following steps in sequence: continuous wire drawing, weaving and post-processing steps, wherein the post-processing steps include acid leaching, thermal cleaning, drying and high-temperature sintering.
[0009] Preferably, in the acid leaching process, the acid solution is sulfuric acid, the acid solution concentration is 2.4±0.4 mol / L, the acid solution temperature is controlled at 90±3°C, and the acid leaching time is 180±10 min.
[0010] The advantages of the present invention are: glass fiber cloth is made by using the existing mature and cost-effective binary system glass fiber production process, and the acid leaching process is used to remove Na2O in the binary system, and the microporous structure formed on the glass fiber cloth is controlled, so that the glass fiber cloth has the characteristics of low dielectric constant. It is achieved without the need for a complex and difficult-to-control ternary system, thereby overcoming technical barriers, replacing imported products, meeting market demand, and reducing the cost of use. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 This is an overall slice diagram of the PCB substrate sample after thermal stress testing in the present invention.
[0012] Figure 2 This is an enlarged view of the upper hole slice of the PCB substrate sample after the thermal stress test in the present invention.
[0013] Figure 3 This is an enlarged view of the lower hole slice after the thermal stress test of the PCB substrate sample in the present invention.
[0014] Figure 4 This is the S parameter of the first sample of the PCB substrate sample of the present invention under 5G.
[0015] Figure 5 This is the S parameter of the first sample of the PCB substrate sample of the present invention under 6G.
[0016] Figure 6 This is the S parameter of the second sample of the PCB substrate sample of the present invention under 5G.
[0017] Figure 7 This is the S parameter of the second sample of the PCB substrate sample of the present invention under 6G. DETAILED DESCRIPTION
[0018] The low dielectric performance glass fiber cloth of the present invention is woven from glass fiber yarn, wherein the glass fiber yarn is a nanosilicate glass fiber and is subjected to acid leaching treatment after weaving so as to remove Na2O in the glass fiber yarn.
[0019] The low dielectric glass fiber cloth comprises at least the following steps in sequence: continuous wire drawing, weaving and post-processing steps, wherein the post-processing steps include acid leaching, thermal cleaning, drying and high-temperature sintering.
[0020] Example 1
[0021] This embodiment exemplifies a manufacturing process for low dielectric glass fiber cloth, and the steps are as follows:
[0022] First, the glass fiber filaments are made by the pool kiln method. The raw materials include quartz sand, weighing 620-660kg, soda ash 300-320kg, nepheline 65-90kg, and small materials 8-10kg. The melting temperature is 1500-1550℃, and the wire drawing temperature is 1280-1320℃ for continuous wire drawing.
[0023] Then, the conventional unwinding and warping process is used to make the plied glass fiber yarn, which is then woven into glass fiber cloth after warping. The parameters are: warp yarn ECE225 1 / 0, weft yarn ECE225 1 / 0, density warp yarn 60±2ends / in, density weft yarn 58±2ends / in, standard weight 105±3g / m 2 , thickness 0.100±0.012mm, air permeability 600~900mm / s, tissue structure wield plain weave,
[0024] Then the post-processing process is carried out, which includes acid leaching, thermal cleaning, drying treatment, and high-temperature sintering. In the acid leaching process, the acid solution is sulfuric acid, and the acid solution concentration is 2.4±
[0025] 0.4mol / L, the acid temperature is controlled at 90±3℃, and the acid leaching time is 180±10min. The acid and impurities on the glass fiber are removed by hot water washing and then dried.
[0026] Finally, sintering is carried out at a sintering temperature of 650-750°C and a sintering furnace line speed of about 2 meters per minute.
[0027] Example 2
[0028] Whether the final performance of the low dielectric glass fiber cloth meets the requirements, the most critical thing is to test and verify it through the final product made of the low dielectric glass fiber cloth, and it must meet the PCB production process requirements.
[0029] First, low-dielectric glass fiber cloth is produced, and then it is made into PP sheets (semi-cured sheets) and CCL (copper clad laminates), and PCB samples are made through ordinary PCB processes. Then, relevant tests are carried out on the PCB samples to confirm whether they can meet the design requirements, thereby proving whether they can replace imported low-dielectric glass fiber cloth in the above-mentioned applications, thereby reducing costs and localizing materials.
[0030] To make PCB samples, you need to first use 2116 low-dielectric glass fiber cloth to make 2116 prepreg, and then use 2116 prepreg to make CCL (copper clad laminate). After the DES process, you will get the inner layer circuit board, and then stack and press several inner layer circuit boards with the prepreg to get the PCB substrate sample.
[0031] The method of Example 1 was used to produce a single weight of 100±2g / m 2 The 2116 low dielectric performance glass fiber cloth uses the same resin formula and dipping process as the same type of glass fiber cloth produced by Japan's Shuber. The 2116 prepreg is produced using high-speed special low-profile 18μm copper foil and is pressed using a German Rafa 6-opening press to produce high-speed CCL.
[0032] The specific process parameters are as follows:
[0033] (1) The resin formula adopts a modified polyphenylene ether resin system for high-speed panels, and the glue index control is: inspection item GT(s) 171°C, index 285.
[0034] (2) The dipping process uses a 10m high oven vertical FR-4 wet dipping machine from Yatai Metal of Taiwan, China.
[0035] (3) Control indicators of prepreg: Prepreg type 2116, unit weight 225g / m 2 , gelation time 200s, fluidity 21%. Production parameters of prepreg: oil temperature in zone 1: 150℃ on top, 130℃ on bottom; oil temperature in zone 2: 150℃ on the left, 150℃ in the middle, 150℃ on the right, vehicle speed 4.0m / min.
[0036] (5) In high-speed CCL production, the cushioning material is 10 sheets of kraft paper on the top and bottom, and the curing condition in the lamination process is 200℃ / 90min.
[0037] The high-speed CCL obtained in the above embodiment 2 was used for testing, and the test data are as follows:
[0038]
[0039] Compared with the imported CCL of the same model of a certain brand on the market, the high-speed CCL obtained by using the above-mentioned embodiment 2 has no obvious difference in Dk / Df. The Dk / Df of the high-speed CCL of this embodiment and the CCL of a certain brand are 3.32 / 0.0046 and 3.68 / 0.0036 respectively.
[0040] Example 3
[0041] The PCB substrate sample is made by using the prepreg and high-speed CCL in the above-mentioned embodiment 2. In this embodiment, the stacking structure of the PCB substrate sample is 2116 prepreg, inner circuit board, 2116 prepreg*2, inner circuit board, 2116 prepreg*2, inner circuit board, 2116 prepreg from top to bottom.
[0042] The specification of 2116 prepreg is 2116, the cutting size is 304*374mm, the specification of inner layer circuit board is 0.254mm H / H, the cutting size is 300*370mm.
[0043] PCB substrate sample process flow: inner layer cutting - inner layer graphics - inner layer etching - inner layer AOI - browning - typesetting - pressing - gong edge after pressing - drilling - plasma - grinding - copper plating - thickening copper - outer layer graphics - outer layer copper etching - outer layer AOI - electrical testing - gold plating - CNC milling - visual inspection - FQA - packaging - shipment.
[0044] The main process parameters are as follows:
[0045] Inner layer etching: Layers L2 / 3, L4 / 5, L6 / 7, temperature 50.5°C, first stage pressure 2.8 / 2.1kg / cm 2 , the first stage pressure is 2.8 / 2.1kg / cm 2 , speed 5000mm / min.
[0046] Pressing: After browning, bake the plate at 110℃*120min, and press it using a burkle press.
[0047] Drilling: Produced using melamine pads and made with Hitachi drilling rigs.
[0048] Copper deposition: plasma degumming is used.
[0049] Outer layer etching: layer type GTL / GBL, temperature 50.8℃, first stage pressure 2.8 / 2.1kg / cm 2 , the first stage pressure is 2.8 / 2.1kg / cm 2 , speed 2200mm / min.
[0050] The other parameters are common PCB process parameters and will not be described in detail here.
[0051] The PCB substrate sample obtained in the above embodiment 3 was used to conduct the finished product reliability test: tin immersion test, temperature 288±5°C, 10s*3 times. And the slice observation was carried out (see Figures 1 to 3 ),from Figures 1 to 3 It can be seen that there is no abnormality such as bursting board, delamination, lack of glue, etc.
[0052] The PCB substrate sample obtained in the above embodiment 3 and a PCB substrate using imported CCL on the market were subjected to moisture resistance test and thermal cycle test respectively. The test method refers to the IPC-TM-650 2.6.3 "Printed Circuit Board Moisture Resistance and Insulation Internal Resistance" test standard and the IPC-TM-650 2.6.6 "Printed Circuit Board Temperature Cycle" test standard.
[0053] Humidity resistance test conditions:
[0054] 1.1 Place the specimens vertically in the test chamber and apply 100V DC to all specimens.
[0055] 1.2 The temperature was adjusted to 50°C, the humidity was set to 93% RH, and the residence time was 168 hours (7 days).
[0056] 1.3 Disconnect the DC voltage and restore the temperature to normal.
[0057] 1.4 After the sample is taken out of the chamber, measure its standing wave ratio in 5G and 6G environments.
[0058] The standing wave ratio test parameter table is as follows:
[0059]
[0060] Conclusion: From the above table, it can be seen that the PCB substrate sample of the present invention and a PCB substrate using imported CCL have a standing wave ratio less than 1.5, both meet the consistency of circuit processing and substrate, and are qualified. However, the PCB substrate sample of the present invention has a greater impact as the frequency increases.
[0061] Thermal cycle test conditions:
[0062] 2.1 Take two small samples of different shapes from the PCB substrate sample for separate testing and place them vertically in the test chamber.
[0063] 2.2 Temperature setting: Step 1: 125℃, time 30min; Step 2: 25℃, time 15min; Step 3: -65℃, time 30min; Step 4: 25℃, time 15min.
[0064] 2.3 From step 1 to step 4 is one cycle, for a total of 500 cycles.
[0065] 2.4 Return the two samples to room temperature, test them separately according to the test items, and measure the S parameters in 5G and 6G environments.
[0066] from Figures 4 to 7 It can be seen that the simulation test results indicate that the low dielectric glass fiber cloth of the present invention has qualified compatibility and reliability with other materials during processing.
[0067] In summary, the low dielectric glass fiber cloth of the present invention can be used for the production of high-speed CCL, and performs well in the PCB process, and can meet the requirements of the PCB production process.
Claims
1. A low dielectric glass fiber cloth, characterized in that: The low dielectric glass fiber cloth is woven from glass fiber yarns, which are nanosilicate glass fibers and are acid leached after weaving.
2. The low dielectric properties glass fiber cloth according to claim 1, characterized in that: The low dielectric glass fiber cloth comprises at least the following steps in sequence: continuous wire drawing, weaving and post-processing steps, wherein the post-processing steps include acid leaching, thermal cleaning, drying and high-temperature sintering.
3. The low dielectric glass fiber cloth according to claim 2, characterized in that: In the acid leaching process, the acid solution is sulfuric acid, the acid solution concentration is 2.4±0.4 mol / L, the acid solution temperature is controlled at 90±3°C, and the acid leaching time is 180±10 min.
Citation Information
Patent Citations
Process for aftertreatment of whole roll of glass fiber grey cloth
CN105133233A
High-silica glass fiber cloth and preparation method thereof
CN116876170A
Glass cloth having low permittivity
JP2003041486A