Bio-based film softener and preparation method thereof
Bio-based softener prepared by bio-based oils and polyethylene polyamines under specific conditions solves the problems of environmental pollution and not easy to degrade by traditional softener, provides environmentally friendly and degradable softener, and improves the quality of textiles and Added value.
Patent Information
- Application Number
- CN202411107114.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-08
AI Technical Summary
The existing soft film softeners are mainly made of petrochemical raw materials, which leads to environmental pollution and is not easy to degrade, making it difficult to meet low-carbon environmental protection standards.
Using bio-based oils and polyethylene polyamines as the main raw materials, deglyceride and dehydration reactions are carried out through a hypophosphite catalyst at specific temperatures and vacuum conditions to form bio-based fatty amide imidazolines, then quaternized and acidified, and finally added bio- Based emulsifier and hand-assisted lifting agent, a bio-based softening agent is prepared.
The prepared bio-based softener has good softness and fluffy feel, is environmentally friendly and degradable, and has a simple and controllable process. It is suitable for mass production, and is more environmentally friendly and sustainable than traditional petrochemical raw materials.
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of textiles, and in particular to a bio-based soft film softener and a preparation method thereof. Background Art
[0002] As a key link in printing and dyeing, soft finishing is essential to improving the hand quality of textiles. During the processing, textiles will become rough due to multiple treatments, especially synthetic fibers and microfiber fabrics. In order to give fabrics a soft, smooth and comfortable touch, the use of softeners becomes particularly important, and softener treatment technology is currently widely used.
[0003] Softener is a chemical that can adjust the static and dynamic friction coefficients of fibers. Reducing the static friction coefficient can make the fiber surface smoother and easier to slide on the fabric; while reducing the dynamic friction coefficient helps the microstructure between fibers to move more easily, making the fibers or fabrics easier to deform, thus making the overall feel softer. Therefore, softeners play an important role in textile finishing. Currently, commonly used softeners include silicone emulsions, soft films, and wax emulsions.
[0004] Soft film is widely used in the post-printing and dyeing finishing stage due to its low price. It can not only improve the quality and added value of textiles, giving them softness, fluffy, elasticity, smoothness, antistatic, antibacterial, anti-ozone and other characteristics, but also optimize the dyeing and finishing process to achieve energy saving and consumption reduction. However, the role of soft film in improving the overall level of the textile industry is indispensable.
[0005] At present, most film softeners are synthesized from petrochemical raw materials. This process consumes a lot of fossil energy and produces emissions such as carbon dioxide, which burdens the environment. It is not easy to degrade in nature and does not meet the requirements of low-carbon environmental protection. Therefore, it is urgent to develop a film softener with simple preparation process, easy degradation, and green environmental protection standards and its preparation method. Summary of the invention
[0006] The purpose of the present application is to provide a bio-based film softener and a preparation method thereof, so as to solve the technical problems that the existing film softeners are derived from petrochemical products, are not easily degradable and are unfavorable to the environment.
[0007] The present application provides a method for preparing a bio-based film softener, comprising the following preparation steps:
[0008] S1. Under the action of hypophosphorous acid catalyst, bio-based oil and polyethylene polyamine are mixed, the temperature is raised to 190-205° C., and a deglycerol reaction is performed to obtain bio-based fatty amide;
[0009] S2, heating the bio-based fatty amide obtained in step S1 to 210-230° C. to perform a dehydration reaction to obtain a bio-based fatty amide imidazoline;
[0010] S3, cooling to 80-100° C., adding diethyl sulfate to the bio-based fatty amide imidazoline obtained in step S2, and then keeping warm for 3-5 hours, adjusting the pH to 6-8 with acetic acid to obtain bio-based fatty amide imidazoline quaternary ammonium salt.
[0011] S4, cooling to 70-80°C, adding bio-based emulsifier and bio-based hand feel auxiliary enhancer to the bio-based fatty amide imidazoline quaternary ammonium salt obtained in step S3, stirring for 2-4 hours, then cooling to 50°C, discharging and slicing to obtain the product bio-based soft film softener.
[0012] Preferably, in step S1, the molar ratio of bio-based oil to polyethylene polyamine is 1:(1.0-3.0); the amount of hypophosphorous acid added is 0.5-1.5% of the total mass of the bio-based oil and polyethylene polyamine.
[0013] Preferably, in step S1, the deglycerolization reaction is carried out under a vacuum degree of -0.1 to -0.08 MPa for 4 to 6 hours, and in step S2, the dehydration reaction is carried out under a vacuum degree of -0.1 to -0.08 MPa for 2 to 4 hours.
[0014] Preferably, in step S3, the molar ratio of polyethylene polyamine to diethyl sulfate is 1:(0.8-1.0);
[0015] Preferably, in step S4, the bio-based emulsifier accounts for 5-9% of the total mass of all raw materials, and the bio-based hand feel auxiliary enhancer accounts for 10-20% of the total mass of all raw materials.
[0016] Preferably, the bio-based oil is one or more of palm oil, palm kernel oil and shortening.
[0017] Preferably, the polyethylene polyamine is one or more of diethylenetriamine, triethylenetetramine and tetraethylenepentamine.
[0018] Preferably, the bio-based emulsifier is one or more of cardanol polyoxyethylene ether, coconut alcohol polyoxyethylene ether, and oleyl alcohol polyoxyethylene ether.
[0019] Preferably, the bio-based hand feel auxiliary enhancing agent is one or more of squalane, sodium hyaluronate, and jojoba oil.
[0020] The present application provides a bio-based soft film softener obtained according to the preparation method of the above-mentioned bio-based soft film softener.
[0021] Therefore, the present application adopts the above-mentioned bio-based film softener and its preparation method, with bio-based oil and polyethylene polyamine as the main raw materials, hypophosphorous acid as the catalyst, ester exchange reaction at 190-220°C to deglycerol to form bio-based fatty amide, and then vacuum dehydration at 210-230°C to synthesize bio-based fatty amide imidazoline, and then quaternization and acidification, and finally adding bio-based emulsifier and bio-based hand feel auxiliary enhancer to obtain the product, which has the following beneficial effects:
[0022] (1) Most of the raw materials of the product of the present invention are derived from natural organisms, with good biodegradability, green and environmental protection, and sustainability. At the same time, the film softener obtained by the present invention is a quaternary ammonium salt type cationic film, which can provide a good soft and fluffy feel, improve the quality of textiles, and increase the added value of fabric products. The component ratio of the present invention is reasonable, and it does not contain environmentally prohibited components such as APEO, and has an excellent soft and fluffy feel.
[0023] (2) The preparation method has simple process steps, high process controllability, low requirements on production equipment, and is suitable for mass production. DETAILED DESCRIPTION
[0024] Example 1
[0025] (1) Using hypophosphorous acid as a catalyst, diethylenetriamine was added to palm oil, the temperature was raised to 190°C, and deglycerol was carried out under a vacuum condition of -0.1MPa for 4 hours to obtain palmitic acid amide; the temperature was raised to 210°C, and dehydrated under a vacuum condition of -0.1MPa for 2 hours to obtain palmitic acid amide imidazoline. The molar ratio of palm oil to diethylenetriamine was 1:1, and the amount of hypophosphorous acid added was 0.5% of the total mass of palm oil and diethylenetriamine;
[0026] (2) cooling to 80° C., adding diethyl sulfate to the palmitic acid amide imidazoline obtained in step (1), and keeping the temperature for 5 hours, wherein the molar ratio of diethylenetriamine to diethyl sulfate is 1:0.8; finally, adjusting the pH to 6 with a small amount of acetic acid to obtain palmitic acid amide imidazoline quaternary ammonium salt;
[0027] (3) Cooling to 70° C., adding cardanol polyoxyethylene ether and squalane to palmitic acid amide imidazoline quaternary ammonium salt, wherein cardanol polyoxyethylene ether accounts for 5% of the total material mass ratio, and squalane accounts for 10% of the total material mass ratio. After stirring for 2 hours, cooling to 50° C., discharging, slicing, and obtaining a product bio-based soft film softener, the yield of the target product is 84%.
[0028] Example 2
[0029] (1) Using hypophosphorous acid as a catalyst, triethylenetetramine was added to palm kernel oil, the temperature was raised to 200°C, and the deglycerol reaction was carried out under a vacuum condition of -0.09 MPa for 5 hours to obtain palm kernel oleic acid amide; the temperature was raised to 220°C, and the dehydration was carried out under a vacuum condition of -0.09 MPa for 3 hours to obtain palm kernel oleic acid amide imidazoline. The molar ratio of palm kernel oil to triethylenetetramine was 1:2, and the amount of hypophosphorous acid added was 1% of the total mass of palm kernel oil and triethylenetetramine;
[0030] (2) cooling to 90° C., adding diethyl sulfate to the palm kernel oleic acid amide imidazoline obtained in step (1), and keeping the temperature for 4 hours, wherein the molar ratio of triethylenetetramine to diethyl sulfate is 1:0.9; finally, adjusting the pH to 7 with a small amount of acetic acid to obtain palm kernel oleic acid amide imidazoline quaternary ammonium salt;
[0031] (3) Cooling to 75° C., adding coconut oil polyoxyethylene ether and sodium hyaluronate to palm kernel oleic acid amide imidazoline quaternary ammonium salt, coconut oil polyoxyethylene ether accounting for 7% of the total material mass ratio, sodium hyaluronate accounting for 15% of the total material mass ratio, stirring for 3 hours, cooling to 50° C., discharging, slicing, and obtaining a product bio-based soft film softener, and the yield of the target product is 87%.
[0032] Example 3
[0033] (1) Using hypophosphorous acid as a catalyst, tetraethylene pentamine is added to shortening, the temperature is raised to 220°C, and deglycerol is reacted for 6 hours under a vacuum condition of -0.08 MPa to obtain shortening acid amide; the temperature is raised to 230°C, and dehydrated for 2 to 4 hours under a vacuum condition of -0.08 MPa to obtain shortening acid amide imidazoline. The molar ratio of shortening to tetraethylene pentamine is 1:3, and the amount of hypophosphorous acid added is 1.5% of the total mass of shortening and tetraethylene pentamine;
[0034] (2) cooling to 100° C., adding diethyl sulfate to the shortening acid amide imidazoline obtained in step (1), and keeping the temperature for 3 hours, wherein the molar ratio of tetraethylenepentamine to diethyl sulfate is in the range of 1:1; finally, adjusting the pH to 8 with a small amount of acetic acid to obtain shortening acid amide imidazoline quaternary ammonium salt;
[0035] (3) cooling to 80° C., adding oleyl alcohol polyoxyethylene ether and jojoba oil to shortening acid amide imidazoline quaternary ammonium salt, wherein oleyl alcohol polyoxyethylene ether accounts for 9% of the total material mass ratio, and jojoba oil accounts for 20% of the total material mass ratio. After stirring for 4 hours, cooling to 50° C., discharging, slicing, and obtaining a product bio-based soft film softener, the yield of the target product is 90%.
[0036] Comparative Example 1
[0037] (1) Using KOH aqueous solution as a catalyst, diethylenetriamine was added to palm oil, the temperature was raised to 190°C, and the deglycerol reaction was carried out under a vacuum condition of -0.1MPa for 4 hours to obtain palmitic acid amide; the temperature was raised to 210°C, and the palmitic acid amide was dehydrated under a vacuum condition of -0.1MPa for 2 hours to obtain palmitic acid amide imidazoline. The molar ratio of palm oil to diethylenetriamine was 1:1, and the amount of hypophosphorous acid added was 0.5% of the total mass of palm oil and diethylenetriamine;
[0038] (2) cooling to 80° C., adding diethyl sulfate to the palmitic acid amide imidazoline obtained in step (1), and keeping the temperature for 5 hours, wherein the molar ratio of diethylenetriamine to diethyl sulfate is 1:0.8; finally, adjusting the pH to 6 with a small amount of acetic acid to obtain palmitic acid amide imidazoline quaternary ammonium salt;
[0039] (3) Cooling to 70° C., adding cardanol polyoxyethylene ether and squalane to palmitic acid amide imidazoline quaternary ammonium salt, wherein cardanol polyoxyethylene ether accounts for 5% of the total material mass ratio, and squalane accounts for 10% of the total material mass ratio. After stirring for 2 hours, cooling to 50° C., discharging, slicing, and obtaining a product bio-based soft film softener, the yield of the target product is 73%.
[0040] Test Example 1
[0041] The cationic film S200 produced by our company and comparative example 1 were selected as comparative samples.
[0042] The samples of Examples 1, 2, 3 and the comparative example were added into normal temperature water at a ratio of 1:9, and diluted to form a dispersion.
[0043] Select pure cotton and white woven fabric, use 50g / L of soft film after dilution at 1:9, and treat the fabric by padding process, and compare the feel and whiteness after finishing.
[0044] Application process: two dips and two rolls (liquid content 65%) → drying → shaping (cotton: 160℃x60s) → moisture regain 3h → comparative test.
[0045] The hand feel is determined by the average of 5 people's evaluations, with 5 being the highest score and 1 being the lowest score. The higher the score, the softer and fluffier the hand feel, and the lower the score, the worse the hand feel.
[0046] The whiteness value is measured by a whiteness meter, and ten points in different areas are selected and the average value is obtained. The higher the whiteness value, the smaller the yellowing and color change value, and the smaller the impact on the color of the dyed fabric.
[0047] Please refer to Table 1 below for the experimental results.
[0048] Table 1 Results
[0049] Film Feel Whiteness Contact angle Example 1 4.5 98.3 39° Example 2 4.5-5 98.6 36° Example 3 5 98.7 37° Comparative Example S200 4.5 96.5 40° Comparative Example 1 3.9 90.1 52°
[0050] It can be seen from the data in the above table that the product produced with bio-based raw materials has the same or better hand feel than the control example; the whiteness of the embodiment is significantly better than that of the control example, that is, the yellowing is significantly less than that of the control example; this shows that the bio-based raw materials described in the present invention can completely replace petrochemical raw materials to produce a more environmentally friendly and sustainable softener, while also having a better hand feel and lower yellowing.
[0051] Therefore, the present application adopts the above-mentioned bio-based film softener and its preparation method to solve the technical problems that the existing film softeners are derived from petrochemical products, are not easy to degrade and are unfavorable to the environment.
[0052] In the description of this specification, the description of reference terms such as "an experimental example", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the experimental example or example are included in at least one experimental example or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same experimental example or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more experimental examples or examples in a suitable manner.
[0053] Finally, it should be noted that the above experimental examples are only used to illustrate the technical solution of the present application rather than to limit it. Although the present application has been described in detail with reference to the preferred experimental examples, ordinary technicians in this field should understand that they can still modify or replace the technical solution of the present application with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present application.
Claims
1. A method for preparing a bio-based film softener, characterized in that: The method comprises the following preparation steps: S1. Under the action of hypophosphorous acid catalyst, bio-based oil and polyethylene polyamine are mixed, the temperature is raised to 190-205° C., and a deglycerol reaction is performed to obtain bio-based fatty amide; S2, heating the bio-based fatty amide obtained in step S1 to 210-230° C. to perform a dehydration reaction to obtain bio-based fatty amide imidazoline; S3, cooling to 80-100° C., adding diethyl sulfate to the bio-based fatty amide imidazoline obtained in step S2, and then keeping warm for 3-5 hours, adjusting the pH to 6-8 with acetic acid to obtain bio-based fatty amide imidazoline quaternary ammonium salt. S4, cooling to 70-80°C, adding bio-based emulsifier and bio-based hand feel auxiliary enhancer to the bio-based fatty amide imidazoline quaternary ammonium salt obtained in step S3, stirring for 2-4 hours, then cooling to 50°C, discharging and slicing to obtain the product bio-based soft film softener.
2. The method for preparing a bio-based film softener according to claim 1, characterized in that: In step S1, the molar ratio of bio-based oil to polyethylene polyamine is 1:(1.0-3.0); the amount of hypophosphorous acid added is 0.5-1.5% of the total mass of the bio-based oil and polyethylene polyamine.
3. A textile-aggregated drug according to claim 1, characterized in that: In step S1, the deglycerol reaction is carried out under a vacuum degree of -0.1 to -0.08 MPa for 4 to 6 hours. In step S2, the dehydration reaction is carried out under a vacuum degree of -0.1 to -0.08 MPa for 2 to 4 hours.
4. The method for preparing a bio-based film softener according to claim 1, characterized in that: In step S3, the molar ratio of polyethylene polyamine to diethyl sulfate is 1:(0.8-1.0).
5. The method for preparing a bio-based film softener according to claim 1, characterized in that: In step S4, the bio-based emulsifier accounts for 5-9% of the total mass of all raw materials, and the bio-based hand feel auxiliary enhancer accounts for 10-20% of the total mass of all raw materials.
6. The method for preparing a bio-based film softener according to claim 1, characterized in that: The bio-based oil is one or more of palm oil, palm kernel oil and shortening.
7. The method for preparing a bio-based film softener according to claim 1, characterized in that: The polyethylene polyamine is one or more of diethylenetriamine, triethylenetetramine and tetraethylenepentamine.
8. The method for preparing a bio-based film softener according to claim 1, characterized in that: The bio-based emulsifier is one or more of cardanol polyoxyethylene ether, coconut alcohol polyoxyethylene ether, and oleyl alcohol polyoxyethylene ether.
9. The method for preparing a bio-based film softener according to claim 1, characterized in that: The bio-based hand feel auxiliary enhancing agent is one or more of squalane, sodium hyaluronate and jojoba oil.
10. The bio-based film softener obtained by the method for preparing a bio-based film softener according to any one of claims 1 to 9.
Citation Information
Cited By
Environment-friendly silk soaking agent and preparation method thereof
CN119352290A
Environmentally friendly silk soaking agent and preparation method thereof
CN119352290B
Low-temperature soluble environment-friendly softening agent as well as preparation method and application thereof
CN122355981A