Antibacterial flame-retardant nylon 66 fiber based on interface epiphytic and preparation method thereof

Through interfacial epiphyseal technology, zinc salt and DTPMPA are combined with cellulose nanocrystalline CNC and embedded in nylon 66 fibers, solving the problems of flammable and insufficient antibacterial performance of nylon 66 fibers, achieving efficient improvement of antibacterial flame retardant performance, suitable for Development of multifunctional high-performance materials.

CN118910886AActive Publication Date: 2024-11-08ZHEJIANG SCI-TECH UNIV +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411083996.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-08
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

Nylon 66 fiber is flammable and produces droplets and toxic gases during combustion, which limits its application. The existing flame retardants have problems such as toxicity, contamination, single function, and compatibility, making it difficult to improve flame retardant performance at the same time. and antibacterial properties.

Method used

Using interfacial epitrophic technology, zinc salt and diethylenetriamine pentamethylphosphonic acid DTPMPA are combined with cellulose nanocrystalline CNC to form the flame retardant DCNC-Zn, which is embedded in nylon 66 fibers through soaking and drying processes to achieve Improved antibacterial flame retardant performance.

Benefits of technology

It realizes excellent antibacterial and flame retardant of nylon 66 fiber, and is non-toxic and pollution-free. It is suitable for military industry, aerospace and other fields, and provides lightweight and high-function components, and is simple and easy to mass production, environmentally friendly and pollution-free.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910886A_ABST
    Figure CN118910886A_ABST
Patent Text Reader

Abstract

The invention relates to an antibacterial flame-retardant nylon 66 fiber based on interface epiphysis and a preparation method thereof, and the preparation method comprises the following steps: (1) adding a zinc salt into a cellulose nanocrystal CNC dispersion liquid, and fully stirring to obtain a uniform CNC-Zn < 2 + > suspension liquid; (2) under the stirring condition, diethylenetriaminepenta (methylene phosphonic acid) DTPMPA is dropwise added into the CNC-Zn < 2 + > suspension liquid, stirring is performed for 60-120 min at the room temperature, and then purification, washing and freeze drying are performed to obtain a flame retardant DCNC-Zn; and (3) soaking the nylon 66 fiber in the DCNC-Zn suspension, and then repeatedly drying and carrying out an interface epiphytic reaction until all the flame retardants are embedded into the nylon 66 fiber to obtain the bacterial flame-retardant nylon 66 fiber. The antibacterial flame-retardant nylon 66 fiber disclosed by the invention has excellent flame-retardant performance and antibacterial performance, has good durability and stability, and has a wide application prospect in the fields of spinning, aviation, packaging and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flame retardant materials, and specifically relates to an antibacterial flame retardant nylon 66 fiber based on interface attachment and a preparation method thereof. Background Art

[0002] Nylon 66 is an indispensable thermoplastic textile fiber that is widely used due to its excellent mechanical properties, thermal stability, chemical stability and wear resistance. However, nylon 66 is very flammable and produces droplets and toxic gases during combustion, which limits its wide application. In addition, nylon 66 also needs to be given antibacterial properties to enhance the multifunctional applicability of the material. Therefore, improving the flame retardant properties of nylon 66 and increasing its versatility are of irreplaceable significance for its application under extreme conditions.

[0003] At present, the flame retardant of nylon 66 is mainly processed by post-finishing, copolymerization and blending. Among them, the post-finishing method is relatively simple, efficient and easy to promote, and is widely used in the flame retardant treatment of nylon 66 yarn and fabric. The flame retardants used for flame retardant modification of nylon 66 can be divided into halogen flame retardants, organic flame retardants, inorganic flame retardants and organic-inorganic hybrid flame retardants according to their composition properties. Halogen flame retardants are greatly restricted in their use due to their serious toxicity and pollution; organic flame retardants are generally phosphorus-containing and nitrogen-containing organic substances. Organic flame retardants can indeed provide good flame retardant efficiency, but most of them have a single function; although inorganic flame retardants are harmless to the environment, they often require a higher addition amount, and their compatibility will affect the mechanical, crystallization and other properties of the matrix. Organic-inorganic hybrid flame retardants can load functional factors on the basis of high-efficiency organic flame retardants, while solving the problems of flame retardant efficiency, compatibility and functionality. Antimicrobial agents are also divided into two types: organic and inorganic. Compared with the poor drug resistance and heat resistance of organic antimicrobial agents, inorganic antimicrobial agents are undoubtedly a more stable and reliable antimicrobial solution. Summary of the invention

[0004] Based on the above-mentioned deficiencies in the prior art, the object of the present invention is to provide an antibacterial flame-retardant nylon 66 fiber based on interface attachment and a preparation method thereof.

[0005] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0006] A method for preparing antibacterial flame-retardant nylon 66 fiber based on interface attachment comprises the following steps:

[0007] (1) Add zinc salt to the cellulose nanocrystal CNC dispersion and stir thoroughly to obtain a uniform CNC-Zn 2+ Suspension;

[0008] (2) Under stirring conditions, diethylenetriamine penta (methylenephosphonic acid) DTPMPA was added dropwise to the CNC-Zn 2+ The suspension was stirred at room temperature for 60-120 min, and then purified, washed, and freeze-dried to obtain the flame retardant DCNC-Zn;

[0009] (3) The nylon 66 fiber is immersed in the DCNC-Zn suspension, and then dried and subjected to interfacial epitaxial reaction repeatedly until all the flame retardants are embedded in the nylon 66 fiber to obtain the antibacterial flame retardant nylon 66 fiber.

[0010] As a preferred embodiment, in step (1), CNC is carboxylated nanocellulose with a size of 250-400 nm.

[0011] As a preferred embodiment, in step (1), the CNC dispersion is obtained by dispersing CNC in water, with a mass fraction of 0.5-5%.

[0012] As a preferred embodiment, in step (1), the mass ratio of zinc salt to CNC is (1-5):1.

[0013] As a preferred embodiment, in step (1), the zinc salt is zinc chloride or zinc nitrate.

[0014] As a preferred solution, in step (2), CNC-Zn 2+ Medium Zn 2+ The molar ratio of DTPMPA is (0.2-0.5):1.

[0015] As a preferred embodiment, in step (3), the DCNC-Zn suspension is obtained by uniformly dispersing DCNC-Zn in water.

[0016] As a preferred embodiment, in step (3), the mass ratio of nylon 66 fiber to DCNC-Zn is 1:(0.01-0.15).

[0017] The present invention also provides antibacterial and flame-retardant nylon 66 fiber prepared by the preparation method described in any of the above schemes.

[0018] As a preferred solution, the antibacterial and flame-retardant nylon 66 fiber has an inhibition zone diameter of not less than 8 mm and a limiting oxygen index of not less than 30%.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] (1) The present invention uses cellulose, an abundant renewable resource, as raw material to prepare CNC, which has the advantages of strong plasticity, high aspect ratio, strong compatibility, low cost, and green environmental protection. Adding inorganic substances often causes agglomeration problems, thus affecting the preset effect. In the present invention, CNC gives full play to the advantages of large specific surface area and excellent compatibility. 2+ The carrier makes the inorganic matter evenly distributed to achieve the effect of optimizing function.

[0021] (2) The addition of CNC in the present invention can provide sufficient carbon source for the matrix. During combustion, CNC is dehydrated into carbon, and a dense protective carbon layer is generated to cover the surface of the matrix to isolate oxygen from entering and heat transfer.

[0022] (3) The cellulose nanocrystals of the present invention and Zn 2+ Provide value to each other. CNC is used as a carrier to make Zn 2+ Uniform distribution, while Zn 2+ Acts as a catalyst to promote carbonization of CNC.

[0023] (4) The present invention adds Zn 2+ , which not only provides antibacterial properties to the flame retardant, but also plays its role in catalyzing carbonization.

[0024] (5) The DTPMPA added in the present invention is a non-toxic, environmentally friendly and sustainable high-phosphorus substance. This substance expands when burned and is a potential flame retardant with great prospects. In the present invention, DTPMPA undergoes a chelating reaction with metal zinc ions to form a stable complex, achieving a technical breakthrough of "multi-functionality in one" (antibacterial ability, flame retardant ability, carbon forming ability, dispersion ability, and binding ability).

[0025] (6) In the present invention, the flame retardant DCNC-Zn forms a stable "iron triangle structure" during the preparation process, that is, CNC and Zn 2+ Electrostatic adsorption occurs, Zn 2+ Chelation reaction occurs with DTPMPA, and esterification reaction occurs between DTPMPA and CNC.

[0026] (7) The DCNC-Zn functional nano flame retardant prepared by the present invention can give nylon 66 fibers and fabrics excellent antibacterial and flame retardant properties, and is non-toxic, non-polluting, and has no special color. It can realize lightweight high-functional components in the fields of military, aerospace, and industry.

[0027] (7) The present invention innovatively applies the interfacial epitaxial growth process to prepare nylon 66 fibers and fabrics with antibacterial and flame retardant properties.

[0028] (8) The preparation process of the present invention is simple, easy to operate, easy to mass produce, and has a large market demand; it is also environmentally friendly and pollution-free, and has broad practical value. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a thermogravimetric test diagram of cellulose nanocrystals, DTPMPA, and DCNC-Zn functional nano flame retardant according to Example 3 of the present invention;

[0030] Figure 2 This is an infrared detection image of cellulose nanocrystals, DTPMPA, and DCNC-Zn functional nano flame retardant according to Example 3 of the present invention;

[0031] Figure 3 This is a SEM image of nylon 66 fiber of Example 3 of the present invention;

[0032] Figure 4 FR-PA66 of Example 3 of the present invention 3 SEM images of the fibers;

[0033] Figure 5 CNC-Zn in Comparative Example 1 of the present invention 2+ 1 、CNC-Zn 2+ 2 、CNC-Zn 2+ 3 、CNC-Zn 2+ 4 、CNC-Zn 2+ 5 Thermogravimetric test diagram of

[0034] Figure 6 PA66 and FR-PA66 in Comparative Example 3 of the present invention 1 、FR-PA66 2 、FR-PA66 3 、FR-PA66 4 、FR-PA66 5 Flame retardant properties of fibers;

[0035] Figure 7 PA66 and FR-PA66 in Comparative Example 3 of the present invention 1 、FR-PA66 2 、FR-PA66 3 、FR-PA66 4 、FR-PA66 5 Graph of the antimicrobial properties of fibers. DETAILED DESCRIPTION

[0036] The technical solution of the present invention is further explained below through specific embodiments.

[0037] Embodiment 1:

[0038] The method for preparing the antibacterial flame-retardant nylon 66 fiber of this embodiment comprises the following steps:

[0039] (1) Preparation of cellulose nanocrystals CNC

[0040] First, prepare 6 mol / mL hydrochloric acid and 3 mol / mL citric acid, take 30 mL hydrochloric acid and 270 mL citric acid and mix them respectively; add 6 g MCC to the mixed acid, stir at 80°C (speed of 400 r / min) for 4 hours; cool to room temperature after sufficient reaction, and dilute with deionized water; centrifuge, remove the supernatant, repeat the operation until pH = 7, and obtain carboxylated cellulose nanocrystals CNC with a size of 250-400 nm;

[0041] (2) CNC-Zn 2+ Preparation of suspension

[0042] 2.5 g of CNC was dispersed in water and ultrasonicated for 60 min to obtain a CNC suspension with a mass fraction of 4.45%;

[0043] Take 5g ZnCl 2 Dissolve in water to prepare 1 mol / mL ZnCl 2 Solution;

[0044] The CNC suspension was mixed with ZnCl 2 The solution was mixed and stirred at room temperature (speed of 600r / min) for 30min to obtain CNC-Zn 2+ Suspension;

[0045] (3) Preparation of DCNC-Zn

[0046] 12.61 g (50%) of DTPMPA was added dropwise to CNC-Zn 2+ The suspension was stirred at room temperature (speed of 350 r / min) for 60 min to fully react; then purified and washed with ethanol to obtain a DCNC-Zn functional nano flame retardant precipitate; the precipitate was freeze-dried for 48 h and ground into powder.

[0047] (4) Preparation of FR-PA66 fiber

[0048] Take 0.06g DCNC-Zn and disperse it in 20mL water, soak 1.2g nylon 66 fiber in the DCNC-Zn suspension, and then dry it in an oven at 80℃, then immerse and react the interface, and repeat the operation until the flame retardant is completely embedded in the nylon 66 fiber.

[0049] Embodiment 2:

[0050] The method for preparing the antibacterial flame-retardant nylon 66 fiber of this embodiment comprises the following steps:

[0051] (1) Preparation of cellulose nanocrystals CNC

[0052] First, prepare 6 mol / mL hydrochloric acid and 3 mol / mL citric acid, take 30 mL hydrochloric acid and 270 mL citric acid and mix them respectively; add 6 g MCC to the mixed acid, stir at 80°C (speed of 400 r / min) for 4 hours; cool to room temperature after sufficient reaction, and dilute with deionized water; centrifuge, remove the supernatant, repeat the operation until pH = 7, and obtain carboxylated cellulose nanocrystals CNC with a size of 250-400 nm;

[0053] (2) CNC-Zn 2+ Preparation of suspension

[0054] 2.5 g of CNC was dispersed in water and ultrasonicated for 60 min to obtain a CNC suspension with a mass fraction of 4.45%;

[0055] Take 5g ZnCl 2 Dissolve in water to prepare 1 mol / mL ZnCl 2 Solution;

[0056] The CNC suspension was mixed with ZnCl 2 The solution was mixed and stirred at room temperature (speed of 600r / min) for 30min to obtain CNC-Zn 2+ Suspension;

[0057] (3) Preparation of DCNC-Zn

[0058] 10.09 g (50%) of DTPMPA was added dropwise to CNC-Zn 2+ The suspension was stirred at room temperature (speed of 350 r / min) for 60 min to fully react; then purified and washed with ethanol to obtain a DCNC-Zn functional nano flame retardant precipitate; the precipitate was freeze-dried for 48 h and ground into powder.

[0059] (4) Preparation of FR-PA66 fiber

[0060] Take 0.06g DCNC-Zn and disperse it in 20mL water, soak 1.2g nylon 66 fiber in the DCNC-Zn suspension, and then dry it in an oven at 80℃, then immerse and react the interface, and repeat the operation until the flame retardant is completely embedded in the nylon 66 fiber.

[0061] Embodiment 3:

[0062] The method for preparing the antibacterial flame-retardant nylon 66 fiber of this embodiment comprises the following steps:

[0063] (1) Preparation of cellulose nanocrystals CNC

[0064] First, prepare 6 mol / mL hydrochloric acid and 3 mol / mL citric acid, take 30 mL hydrochloric acid and 270 mL citric acid and mix them respectively; add 6 g MCC to the mixed acid, stir at 80°C (speed of 400 r / min) for 4 hours; cool to room temperature after sufficient reaction, and dilute with deionized water; centrifuge, remove the supernatant, repeat the operation until pH = 7, and obtain carboxylated cellulose nanocrystals CNC with a size of 250-400 nm;

[0065] (2) CNC-Zn 2+ Preparation of suspension

[0066] 2.5 g of CNC was dispersed in water and ultrasonicated for 60 min to obtain a CNC suspension with a mass fraction of 4.45%;

[0067] Take 5g ZnCl 2 Dissolve in water to prepare 1 mol / mL ZnCl 2 Solution;

[0068] The CNC suspension was mixed with ZnCl 2 The solution was mixed and stirred at room temperature (speed of 600r / min) for 30min to obtain CNC-Zn 2+ Suspension;

[0069] (3) Preparation of DCNC-Zn

[0070] 8.41 g (50%) of DTPMPA was added dropwise to CNC-Zn 2+ The suspension was stirred at room temperature (speed of 350 r / min) for 60 min to fully react; then purified and washed with ethanol to obtain a DCNC-Zn functional nano flame retardant precipitate; the precipitate was freeze-dried for 48 h and ground into powder;

[0071] (4) Preparation of FR-PA66 fiber

[0072] Take 0.06g DCNC-Zn and disperse it in 20mL water, soak 1.2g nylon 66 fiber in the DCNC-Zn suspension, and then dry it in an oven at 80℃, then immerse and react the interface, and repeat the operation until the flame retardant is completely embedded in the nylon 66 fiber.

[0073] like Figure 1 As shown, the generation and movement of the new peak in DCNC-Zn of this example indicate the occurrence of chelating reaction; Figure 2 As shown in the figure, the residual amount of DCNC-Zn in this example is significantly improved, which fully proves that CNC provides carbon source and Zn 2+ The effect of catalysis into carbon; Figure 3 , Figure 4 As shown in the figure, the surface of nylon 66 fiber is smooth, and after embedding DCNC-Zn functional nano flame retardant, the surface of nylon 66 fiber is rough and has an obvious flame retardant layer.

[0074] Embodiment 4:

[0075] The method for preparing the antibacterial flame-retardant nylon 66 fiber of this embodiment comprises the following steps:

[0076] (1) Preparation of cellulose nanocrystals CNC

[0077] First, prepare 6 mol / mL hydrochloric acid and 3 mol / mL citric acid, take 30 mL hydrochloric acid and 270 mL citric acid and mix them respectively; add 6 g MCC to the mixed acid, stir at 80°C (speed of 400 r / min) for 4 hours; cool to room temperature after sufficient reaction, and dilute with deionized water; centrifuge, remove the supernatant, repeat the operation until pH = 7, and obtain carboxylated cellulose nanocrystals CNC with a size of 250-400 nm;

[0078] (2) CNC-Zn 2+ Preparation of suspension

[0079] 2.5 g of CNC was dispersed in water and ultrasonicated for 60 min to obtain a CNC suspension with a mass fraction of 4.45%;

[0080] Take 5g ZnCl 2 Dissolve in water to prepare 1 mol / mL ZnCl 2 Solution;

[0081] The CNC suspension was mixed with ZnCl 2 The solution was mixed and stirred at room temperature (speed of 600r / min) for 30min to obtain CNC-Zn 2+ Suspension;

[0082] (3) Preparation of DCNC-Zn

[0083] 7.21 g (50%) of DTPMPA was added dropwise to CNC-Zn 2+ The suspension was stirred at room temperature (speed of 350 r / min) for 60 min to fully react; then purified and washed with ethanol to obtain a DCNC-Zn functional nano flame retardant precipitate; the precipitate was freeze-dried for 48 h and ground into powder.

[0084] (4) Preparation of FR-PA66 fiber

[0085] Take 0.06g DCNC-Zn and disperse it in 20mL water, soak 1.2g nylon 66 fiber in the DCNC-Zn suspension, and then dry it in an oven at 80℃, then immerse and react the interface, and repeat the operation until the flame retardant is completely embedded in the nylon 66 fiber.

[0086] Comparative Example 1:

[0087] The antibacterial flame-retardant nylon 66 fiber of this comparative example is different from that of Example 3 in that:

[0088] Study on CNC and ZnCl 2 The effect of different mass ratios on the thermal properties of fibers;

[0089] Add different concentrations of Zn 2+ CNC-Zn 2+ , set CNC and ZnCl 2 The mass ratios are 1:1, 1:2 (i.e., Example 3), 1:3, 1:4, and 1:5 respectively;

[0090] The other steps are the same as in Example 3;

[0091] The antibacterial flame retardant nylon 66 fiber CNC-Zn 2+ 1 , CNC-Zn 2+ 2 , CNC-Zn 2+ 3 , CNC-Zn 2+ 4 , CNC-Zn 2+ 5 The thermal properties of Figure 5 As shown, with the Zn 2+ With the increase of concentration, CNC-Zn 2+ The residual amount of CNC and ZnCl 2 When the mass ratio is greater than 1:2, CNC-Zn 2+ The residual amount of CNC and ZnCl 2 The best mass ratio is 1:2.

[0092] Comparative Example 2:

[0093] The antibacterial flame-retardant nylon 66 fiber of this comparative example is different from that of Example 3 in that:

[0094] The CNC suspension, zinc salt and DTPMPA were directly mixed and reacted, mixed and stirred (rotation speed was 600 r / min) at room temperature for 60 minutes, then purified and washed with ethanol, freeze-dried for 48 hours, and ground into powder to obtain the flame retardant CNC-DTPMPA-Zn.

[0095] Take 0.06g CNC-DTPMPA-Zn and disperse it in 20mL water, soak 1.2g nylon 66 fiber in the DCNC-Zn suspension, and then dry it in an oven at 80℃, and then immerse and react the interface, and repeat the operation until the flame retardant is completely embedded in the nylon 66 fiber to obtain fiber CNC-DTPMPA-Zn-PA66;

[0096] The other steps are the same as in Example 3;

[0097] The LOI of CNC-DTPMPA-Zn-PA66 in this comparative example is only 25.8%, and the flame retardant effect is not obvious. This is because direct mixing will cause Zn 2+ The chelation reaction directly occurs with DTPMPA, and CNC is "squeezed" out of the system. The esterification reaction becomes difficult and random, and eventually an unstable one-, two-, or three-component mixed structure is formed. It is difficult for CNC alone to achieve a flame retardant effect. Without CNC, DTPMPA-Zn 2+ Without the rich carbon source, it is difficult to achieve a good flame retardant effect.

[0098] Comparative Example 3:

[0099] The antibacterial flame-retardant nylon 66 fiber of this comparative example is different from that of Example 3 in that:

[0100] The effects of different embedding amounts of DCNC-Zn functional nano flame retardant on the flame retardant and antibacterial properties of antibacterial flame retardant nylon 66 fiber were studied.

[0101] The nylon 66 fiber PA66 was immersed in different concentrations of DCNC-Zn suspensions, and the embedding amount of DCNC-Zn functional nano flame retardant was 1%, 3%, 5%, 7%, and 9%. The antibacterial flame retardant nylon 66 fibers obtained were FR-PA66, 1 、FR-PA66 2 、FR-PA66 3 (ie, Example 3), FR-PA66 4 、FR-PA66 5 ;

[0102] The other steps are the same as those in Example 3.

[0103] For the above-mentioned fibers PA66, FR-PA66 1 、FR-PA66 2、FR-PA66 3 、FR-PA66 4 、FR-PA66 5 Conduct flame retardant performance tests, such as Figure 5 As shown in Figure 2, with the increase of DCNC-Zn embedding content, the LOI of the fiber increases from 18.3% of pure nylon 66 fiber PA66 to 18.3% of fiber FR-PA66. 3 33.7%. When the DCNC-Zn embedding amount exceeds 5%, the excess nano flame retardant aggregates or easily falls off on the fiber surface, and the LOI value increment is not obvious. It can be concluded that the DCNC-Zn concentration is 5% for the best;

[0104] For the above-mentioned fibers PA66, FR-PA66 1 、FR-PA66 2 、FR-PA66 3 、FR-PA66 4 、FR-PA66 5 Conduct antimicrobial performance tests, such as Figure 6 As shown in Figure 2, with the increase of DCNC-Zn embedding amount, the antibacterial activity of the fiber against Escherichia coli (white column in the figure) and Staphylococcus aureus (grey column in the figure) gradually increased, and the inhibition zone increased from 0 for pure nylon 66 fiber PA66 to 0. 1 3.2mm (S. aureus), 2.9mm (E. coli), and further expanded to fiber FR-PA66 3 When the DCNC-Zn embedding amount exceeds 5%, the excessive nano flame retardant aggregates or falls off easily on the fiber surface, and the expansion of the inhibition zone does not change much. Therefore, the embedding amount of DCNC-Zn is 5%, which is the best.

[0105] In the above embodiment and its alternatives, the mass fraction of the CNC dispersion may also be 0.5%, 1%, 2.5%, 5%, etc.

[0106] In the above embodiment and its alternatives, zinc chloride may also be replaced by zinc nitrate.

[0107] In the above embodiment and its alternatives, the mass ratio of zinc salt to CNC can also be 1.5:1, 2.5:1, 3.5:1, 4.5:1, etc.

[0108] In the above embodiment and its alternatives, DTPMPA and Zn 2+ The ratio of the amounts of substances can also be 1:0.2, 1:0.3, 1:0.4, 1:0.5, etc.

[0109] In the above embodiment and its alternatives, the mass ratio of nylon 66 fiber to DCNC-Zn can also be 1:0.02, 1:0.06, 1:0.1, 1:0.12, 1:0.15, etc.

[0110] The above description is only a detailed description of the preferred embodiments and principles of the present invention. For ordinary technicians in this field, according to the ideas provided by the present invention, there will be changes in the specific implementation methods, and these changes should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing antibacterial flame-retardant nylon 66 fiber based on interface attachment, characterized in that: The following steps are involved: (1) Add zinc salt to the cellulose nanocrystal CNC dispersion and stir thoroughly to obtain a uniform CNC-Zn 2+ Suspension; (2) Under stirring conditions, diethylenetriamine penta (methylenephosphonic acid) DTPMPA was added dropwise to the CNC-Zn 2+ The suspension was stirred at room temperature for 60-120 min, and then purified, washed, and freeze-dried to obtain the flame retardant DCNC-Zn; (3) The nylon 66 fiber is immersed in the DCNC-Zn suspension, and then dried and subjected to interfacial epitaxial reaction repeatedly until all the flame retardants are embedded in the nylon 66 fiber to obtain the antibacterial flame retardant nylon 66 fiber.

2. The preparation method according to claim 1, characterized in that: In the step (1), CNC is carboxylated nanocellulose with a size of 250-400 nm.

3. The preparation method according to claim 2, characterized in that: In the step (1), the CNC dispersion is obtained by dispersing CNC in water, with a mass fraction of 0.5-5%.

4. The preparation method according to claim 1, characterized in that: In the step (1), the mass ratio of zinc salt to CNC is (1-5):

1.

5. The preparation method according to claim 1, characterized in that: In the step (1), the zinc salt is zinc chloride or zinc nitrate.

6. The preparation method according to claim 1, characterized in that: In the step (2), CNC-Zn 2+ Medium Zn 2+ The molar ratio of DTPMPA is (0.2-0.5):

1.

7. The preparation method according to claim 1, characterized in that: In the step (3), the DCNC-Zn suspension is obtained by uniformly dispersing DCNC-Zn in water.

8. The preparation method according to claim 1, characterized in that: In the step (3), the mass ratio of nylon 66 fiber to DCNC-Zn is 1:(0.01-0.15).

9. The antibacterial and flame-retardant nylon 66 fiber obtained by the preparation method according to any one of claims 1 to 8.

10. The antibacterial flame-retardant nylon 66 fiber according to claim 9, characterized in that: The diameter of the inhibition zone is not less than 8mm, and the limiting oxygen index is not less than 30%.

Citation Information

Patent Citations

  • Method for manufacturing zinc oxide-cellulose nanocrystalline composite fiber film with antibacterial characteristic and photocatalytic degradation characteristic at same time

    CN104018235A

  • Bio-based flame retardant as well as preparation method and application thereof

    CN110041565A

  • Diethylenetriaminepenta (methylene phosphonic acid) melamine aluminum salt modified lignin single-component intumescent flame retardant as well as preparation method and application thereof

    CN114196040A

  • Nano-zinc oxide modified flame-retardant antibacterial polyester fiber and preparation method thereof

    CN116262989A

  • Flame retardant with ultrahigh heat-resistant expansibility, preparation method of flame retardant and application of flame retardant nylon fabric

    CN118048786A