MOX-coated GO co-supported graphene transfer composite gas-sensitive film and preparation method thereof
By forming the MOX@GO layer on the graphene layer, the transfer graphene gas-sensitive film is solved, and the problem of electrical performance loss in the improvement of graphene gas-sensitive performance is achieved, and high-efficiency gas detection and structural stability are improved.
Patent Information
- Application Number
- CN202411024488.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-08
AI Technical Summary
Existing graphene gas-sensitive sensors often sacrifice their electrical properties in the process of improving gas-sensitive performance, resulting in increased signal attenuation and circuit design complexity, and structural stability problems exist, limiting their use in practical applications.
Using MOX@GO to co-support the composite gas-sensitive film of transfer graphene, a loose layered nanostructure is formed by setting the graphene oxide sheet layer and the MOX@GO layer with metal oxide nanoparticles on the surface of the graphene layer to form a loose layered nanostructure, providing Gas molecular diffusion channels and adsorption sites, and use the underlying graphene layer to provide high-speed charge transport channels, the film is prepared in combination with ultrasonic dispersion and spin coating technology.
High-efficiency gas detection is achieved, organic matter residues are avoided during graphene transfer, gas-sensitive performance is significantly improved, and the electrical performance of graphene is maintained, overcoming the problem of improving gas-sensitive characteristics but sacrificing electrical performance in the prior art.
Smart Images

Figure CN118914299A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of semiconductor gas sensors and particularly relates to a MO X @GO co-supported transferred graphene composite gas-sensitive film and its preparation method. Background Art
[0002] Gas detection and identification have a wide range of application needs. Future-oriented gas sensors should be miniaturized and highly integrated, which continuously puts forward higher requirements on the size, power consumption and identification ability of sensors. Currently, commercial gas sensors are usually based on metal oxide sensitive materials, which often need to be heated to more than 200 degrees Celsius during the sensing process, resulting in high device energy consumption. Graphene (Gr) grown by chemical vapor deposition (CVD) has high carrier mobility, large specific surface area, and especially room temperature working ability, which has aroused great interest in the field of gas sensing, but the physical adsorption behavior based on van der Waals forces limits the sensitivity and selectivity of graphene to gas.
[0003] Common methods for improving the gas-sensing properties of graphene include surface modification of nanoparticles, surface grafting of functional groups, and surface atomic doping or introduction of defects. However, these methods often involve complex chemical reactions, which leads to cumbersome device preparation processes and sacrifice the excellent electrical properties of graphene (such as high carrier mobility), which in turn leads to problems such as signal attenuation and increased complexity of circuit design, greatly limiting the application of graphene sensors in actual circuits. Another idea is to replace graphene with reduced graphene oxide (rGO) with good conductivity and rich surface oxygen functional groups, but this method has structural stability problems such as sheet agglomeration. Therefore, exploring methods to improve the gas-sensing properties of graphene films is of great significance but still faces great challenges. Summary of the invention
[0004] In order to solve the problems existing in the prior art, the object of the present invention is to provide a MO X The composite gas-sensitive film of @GO co-supported transferred graphene and its preparation method can effectively overcome the technical difficulties of improving the gas-sensitive properties of Gr but sacrificing its electrical properties in current research.
[0005] The technical solution adopted by the present invention is as follows:
[0006] a kind of MO X The composite gas-sensitive film of @GO co-supported transferred graphene includes a graphene layer, and the surface of the graphene layer is provided with MO X @GO layer, the MO X The @GO layer includes graphene oxide sheets and metal oxide nanoparticles attached to the graphene oxide sheets.
[0007] Preferably, the diameter of the graphene oxide sheet is 1 μm-100 μm; the particle size of the metal oxide nanoparticles is 5-50 nm; and the mass ratio of the graphene oxide sheet to the metal oxide nanoparticles is 1:(0.1-10).
[0008] Preferably, the graphene layer is a single-layer graphene or a few-layer graphene.
[0009] Preferably, the metal oxide nanoparticles include at least one of SnO2, ZnO, Co3O4, V2O5, CuO and Fe2O3.
[0010] Preferably, the MO of the present invention X The composite gas-sensitive film of the co-supported transferred graphene of @GO also includes a substrate, which is arranged on the graphene layer and X @The surface opposite to the GO layer.
[0011] The present invention also provides the MO as described above X The preparation method of the composite gas-sensitive membrane of @GO co-supported transferred graphene includes the following steps:
[0012] The metal oxide nanoparticle dispersion is uniformly dispersed in the graphene oxide dispersion, and then ultrasonic dispersion is performed to make the metal oxide nanoparticles adhere to the graphene oxide sheet to form MO X @GO dispersion;
[0013] The MO X @GO dispersion is spin-coated on the prepared graphene layer surface to form MO X @GO@Gr composite structure nanofilm, and then dried to obtain the MO X Composite gas-sensitive film of @GO co-supported transferred graphene.
[0014] Preferably, the metal oxide nanoparticles are first ground and dispersed, and then the ground and dispersed metal oxide nanoparticles are uniformly dispersed in the graphene oxide dispersion.
[0015] Preferably, the concentration of the metal oxide nanoparticle dispersion is 0.1-10 mg / ml; the concentration of the graphene oxide dispersion is 0.1-10 mg / mL, the power of ultrasonic dispersion is 200-400w, and the time is 10-60 minutes.
[0016] Preferably: the MO X When the GO dispersion is spin-coated on the surface of the prepared graphene layer, the spin-coating speed is 100-1000 rpm and the spin-coating time is 1-60 seconds;
[0017] The MO XAfter the @GO dispersion is spin-coated on the surface of the prepared graphene layer, it is dried at a temperature of 80-100° C. and a drying time of 30-300 seconds.
[0018] Preferably: the graphene layer is prepared on the surface of the copper foil substrate;
[0019] The preparation method also includes a process of etching the copper foil substrate: placing the side with the copper foil substrate in an etching solution for etching, removing the copper foil substrate, and then rinsing the remaining part to obtain the MO X @GO co-supported transferred graphene composite gas-sensitive film;
[0020] The solute of the etching solution is FeCl3 or (NH4)2S2O8, the concentration is 1-10 mol / L, and the etching time is 1-5 hours.
[0021] The present invention has the following beneficial effects:
[0022] The present invention MO X The composite gas-sensitive membrane of @GO co-supported transferred graphene is a MO with a nanocomposite structure X @GO@Gr high-performance gas-sensitive film, among which MO X Metal oxide nanoparticles are attached to the GO (graphene oxide) sheets to form a loose layered nanostructure, which provides a maximized gas molecule diffusion channel and effective adsorption sites, while the bottom graphene layer with a complete structure provides a high-speed charge transfer channel. X @GO acts as a gripper to capture gas molecules, and the underlying Gr converts charge changes into resistance signals for rapid detection, thereby achieving efficient gas detection. X @GO is used as a supporting film to effectively avoid the residue of organic matter during the graphene transfer process. The present invention can effectively overcome the technical difficulty of improving the gas-sensitive properties of Gr but sacrificing its electrical properties in current research. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is a transmission electron microscope image of SnO2 nanoparticles used in the embodiment of the present invention;
[0024] Figure 2 is a scanning electron microscope image of GO used in the embodiment of the present invention;
[0025] Figure 3 is a scanning electron microscope image of the SnO2@GO / Gr composite film prepared in Example 1 of the present invention;
[0026] Figure 4 is a scanning electron microscope image of the SnO2@GO@Gr composite film prepared in Example 2 of the present invention;
[0027] Figure 5 is a scanning electron microscope image of the SnO2@GO@Gr composite film prepared in Example 3 of the present invention;
[0028] Figure 6 is a scanning electron microscope image of the SnO2@GO@Gr composite film prepared in Example 4 of the present invention;
[0029] Figure 7 is a scanning electron microscope image of the SnO2@GO@Gr composite film prepared in Example 5 of the present invention;
[0030] Figure 8 is a scanning electron microscope image of the GO@Gr composite film prepared in Comparative Example 1 of the present invention;
[0031] Fig. 9 The dynamic response curves of the SnO2@GO@Gr composite film sensor and the Gr sensor prepared in Example 1, Example 2, Example 3, Example 4, Example 5 and Comparative Example 1 of the present invention to NH3;
[0032] Fig.10 This is a comparison of the gas-sensitive responses of the SnO2@GO@Gr composite film sensor and the Gr sensor prepared in Example 1, Example 2, Example 3, Example 4, Example 5 and Comparative Example 1 of the present invention to NH3. DETAILED DESCRIPTION
[0033] The present invention will be further described below with reference to the accompanying drawings and embodiments.
[0034] The present invention MO X The preparation method of the composite gas-sensitive membrane of @GO co-supported transferred graphene comprises the following steps:
[0035] S1, ultrasonically disperse GO in a suitable solvent to form a stable GO dispersion. The solvent can be water or ethanol. The concentration of the GO dispersion is 0.1-10 mg / mL. The scanning electron microscope image of GO used in the technical solution of the present invention is as follows Figure 5 As shown, it can be seen that the diameter of the graphene oxide sheet is 1 μm-100 μm.
[0036] S2, the nano-MO X Particles are mechanically dispersed to avoid nano-scale MO X Particle agglomeration to enhance nanoscale MO X The interaction between particles and GO. X The particles may be at least one of SnO2, ZnO, Co3O4, V2O5, CuO and Fe2O3. X The particle size is 5-50nm, and the nano-scale MO of the above particle sizeX The particles are advantageously attached to the graphene oxide sheets having the above-mentioned diameter requirements.
[0037] S3, the nano-scale MO treated by S2 X The particles are ultrasonically dispersed in a suitable solvent to form nano-scale MO X Particle dispersion, nano-scale MO X The concentration of the particle dispersion is 0.1-10 mg / ml,
[0038] S4, the above nano-scale MO X The particle dispersion is dispersed in the above GO dispersion, and then ultrasonically dispersed to make nano-MO X The particles are firmly attached to the GO sheets to form MO X @GO dispersion. The power of ultrasonic dispersion is 200-400w, and the time is 10-60 minutes. The mass ratio of graphene oxide sheets to metal oxide nanoparticles is 1:(0.1-10).
[0039] S5, depositing high-performance large-area continuous graphene on a copper foil substrate by chemical vapor deposition, wherein the graphene may be a single-layer or few-layer graphene (few-layer means the number of layers is greater than or equal to 2 and less than or equal to 10).
[0040] S6, the MO prepared in step S4 X @GO dispersion is evenly spin-coated on the graphene surface described in step S5 to form MO X @GO@Gr composite structure nanofilm. The spin coating speed is 100-1000 rpm and the spin coating time is 1-60 seconds.
[0041] S7, drying the device obtained in S6 at 80-100° C. for 30-300 seconds to evaporate the solvent of the dispersion.
[0042] S8, transferring the device obtained in step S7 into an etching solution, with the copper foil substrate at the bottom of the device. The etching solution can be FeCl3 or (NH4)2S2O8 solution, the etching solution concentration is 1-10 mol / L, and the etching time can be 1-5 hours.
[0043] S9, then rinse the device treated in S8 in deionized water, and after rinsing, obtain the MO of the present invention X Composite gas-sensitive film of @GO co-supported transferred graphene.
[0044] MO prepared by the above preparation method of the present invention X The composite gas-sensitive membrane structure of @GO co-supported transferred graphene is as follows: It includes a graphene layer, and the surface of the graphene layer is provided with MO X @GO layer, the MO XThe @GO layer includes graphene oxide sheets and metal oxide nanoparticles attached to the graphene oxide sheets.
[0045] The present invention MO X When the composite gas-sensitive film of @GO co-supported transferred graphene is used as the sensitive layer of the gas-sensitive element, the following steps are also included:
[0046] S10, transferring the composite gas-sensitive membrane obtained in step S9 to the electrode substrate, and then drying it to obtain the MO based on the present invention. X Gas sensor based on composite gas sensitive film of @GO co-supported transferred graphene.
[0047] In the following examples of the present invention, the metal oxide nanoparticles are SnO2, and the following examples also take the preparation of SnO2@GO@Gr gas-sensitive film as an example to illustrate the present invention.
[0048] The synthesis process of metal oxide nanoparticles using SnO2 includes:
[0049] Weigh 50 mg of SnCl4·5H2O, put it into a high-temperature reactor with a polytetrafluoroethylene liner, and add 50 ml of deionized water. Seal the reactor and put it into an oven to react at 180°C for 12 hours. After the reaction is completed, cool the reactor naturally to room temperature. Take out the product in the reactor, wash it alternately with deionized water and anhydrous ethanol 4-5 times, and after drying in an oven, SnO2NPs (i.e. SnO2 nanoparticles) are obtained.
[0050] Example 1
[0051] This embodiment M0 X The preparation method of the composite gas-sensitive membrane of @GO co-supported transferred graphene comprises the following steps
[0052] 1) Weigh a certain amount of the above SnO2 powder and add an appropriate amount of anhydrous ethanol to prepare a SnO2 dispersion with a concentration of 0.1 mg / ml.
[0053] 2) SnO2@GO transfer graphene
[0054] Weigh 20 mg GO, add 20 ml deionized water, shake well, and disperse by ultrasound for 4 hours to obtain a uniform GO dispersion with a concentration of 1 mg / ml. Take 1 mL GO dispersion, add 1 mL SnO2 dispersion prepared in step 1), and then mix by ultrasound for 60 minutes at a power of 200 W. XThe particles are firmly attached to the GO sheet to form a SnO2@GO dispersion. Then the SnO2@GO dispersion is dropped on the grown single-layer copper-based CVD graphene, and the dispersion is spin-coated at 1000 rpm for 1 second using a spin coater, and then quickly dried at 100°C for 30 seconds. The resulting device is cut into 0.5×0.5mm 2 Then, SnO2@GO was placed face up on the surface of 10 mol / L (NH4)2S2O8 solution for 1 hour to etch the copper foil substrate at the bottom of the composite film. When the copper foil substrate was completely etched, the SnO2@GO@Gr composite film was obtained.
[0055] By transferring the SnO2@GO@Gr composite film of this embodiment to an electrode substrate, a gas sensor based on the SnO2@GO@Gr composite film can be obtained.
[0056] like Figure 3 As shown in Figure 2, SnO2@GO is tightly composited with Gr to form a good support layer for Gr transfer. It can be observed that a small amount of SnO2 nanoparticles are attached to the surface of GO.
[0057] like Fig. 9 As shown, it can be seen that the initial resistance value of the gas sensor prepared using the SnO2@GO@Gr composite film of this embodiment is 467Ω, and the initial resistance value of the Gr sensor is 464Ω. The resistance values of the two are close, indicating that SnO2@GO in this embodiment can serve as a good supporting layer to ensure the integrity of Gr during the transfer process.
[0058] like Fig.10 As shown, it can be seen that for any concentration of NH3, the response of the gas sensor prepared using the SnO2@GO@Gr composite film of this embodiment is significantly higher than that of the Gr sensor. For example, for 100ppm NH3, the response of the composite film sensor in this embodiment is 9.86%, which is 3.5 times the response of the Gr sensor (2.80%). This shows that the SnO2@GO@Gr composite structure nanofilm proposed in the present invention has excellent gas sensing performance.
[0059] Example 2
[0060] This embodiment M0 X The preparation method of the composite gas-sensitive membrane of @GO co-supported transferred graphene comprises the following steps
[0061] 1) Weigh a certain amount of the above SnO2 powder and add an appropriate amount of anhydrous ethanol to prepare a SnO2 dispersion with a concentration of 0.5 mg / ml.
[0062] 2) SnO2@GO transfer graphene
[0063] Weigh 20 mg GO, add 20 ml deionized water, shake well, and disperse by ultrasound for 4 hours to obtain a uniform GO dispersion with a concentration of 1 mg / ml. Take 1 mL GO dispersion, add 1 mL SnO2 dispersion prepared in step 1), and then mix by ultrasound for 50 minutes at a power of 250 W. X The particles are firmly attached to the GO sheet to form a SnO2@GO dispersion. Then the SnO2@GO dispersion is dropped on the grown single-layer copper-based CVD graphene, and the dispersion is spin-coated at 800 rpm for 20 seconds using a spin coater, and then quickly dried at 95°C for 50 seconds. The resulting device is cut into 0.5×0.5mm 2 Then, SnO2@GO was placed with the surface facing upwards on the surface of 8 mol / L (NH4)2S2O8 solution for 2 hours to etch the copper foil substrate at the bottom of the composite film. When the copper foil substrate was completely etched, the SnO2@GO@Gr composite film was obtained.
[0064] By transferring the SnO2@GO@Gr composite film of this embodiment to an electrode substrate, a gas sensor based on the SnO2@GO@Gr composite film can be obtained.
[0065] like Figure 4 As shown, it was observed that a certain amount of SnO2 nanoparticles were uniformly attached to the GO surface, together forming a supporting layer for the transferred graphene.
[0066] like Fig. 9 As shown, it can be seen that the initial resistance value of the gas sensor prepared using the SnO2@GO@Gr composite film of this embodiment is 460Ω, which is close to the initial resistance value of the Gr sensor, indicating that SnO2@GO in this embodiment can serve as a good supporting layer to ensure the integrity of Gr during the transfer process.
[0067] like Fig.10 As shown, it can be seen that for any concentration of NH3, the response of the gas sensor prepared using the SnO2@GO@Gr composite film of this embodiment is significantly higher than that of the Gr sensor. For example, for 100ppm NH3, the response of the composite film sensor in this embodiment is 17.11%, which is 6.1 times the response of the Gr sensor (2.80%) and 1.7 times the gas-sensitive response (9.86%) in Example 1. This shows that the SnO2@GO@Gr composite structure nanofilm proposed in the present invention has excellent gas-sensitive properties.
[0068] Example 3
[0069] This embodiment M0 X The preparation method of the composite gas-sensitive membrane of @GO co-supported transferred graphene comprises the following steps
[0070] 1) Weigh a certain amount of the above SnO2 powder and add an appropriate amount of anhydrous ethanol to prepare a SnO2 dispersion with a concentration of 1 mg / ml.
[0071] 2) SnO2@GO transfer graphene
[0072] Weigh 20 mg GO, add 20 ml deionized water, shake well, and disperse by ultrasound for 4 hours to obtain a uniform GO dispersion with a concentration of 1 mg / ml. Take 1 mL GO dispersion, add 1 mL SnO2 dispersion prepared in step 1), and then mix by ultrasound for 35 minutes. The ultrasonic power is set to 300 w to make the nano-MO X The particles are firmly attached to the GO sheet to form a SnO2@GO dispersion. Then the SnO2@GO dispersion is dropped on the grown single-layer copper-based CVD graphene, and the dispersion is spin-coated at 500 rpm for 5 seconds using a spin coater, and dried at 90°C for 100 seconds. The resulting device is cut into 0.5×0.5mm 2 Then, SnO2@GO was placed with the surface facing upwards on the surface of 5 mol / L (NH4)2S2O8 solution for 3 hours to etch the copper foil substrate at the bottom of the composite film. When the copper foil substrate was completely etched, the SnO2@GO@Gr composite film was obtained.
[0073] By transferring the SnO2@GO@Gr composite film of this embodiment to an electrode substrate, a gas sensor based on the SnO2@GO@Gr composite film can be obtained.
[0074] like Figure 5 As shown in the figure, a large number of SnO2 nanoparticles are uniformly attached to the GO surface, forming a supporting layer for the transferred graphene. In addition, the film surface is relatively rough, because the attachment of SnO2 improves the agglomeration of GO sheets, which is beneficial to the diffusion and adsorption of gas molecules on the surface of the sensitive material during the gas sensing test.
[0075] like Fig. 9 As shown, it can be seen that compared with the Gr sensor, the gas sensor prepared using the SnO2@GO@Gr composite film of this embodiment has similar initial resistance values of 468Ω and 464Ω, respectively, indicating that SnO2@GO in this embodiment can serve as a good supporting layer to ensure the integrity of Gr during the transfer process.
[0076] like Fig.10As shown, it can be seen that for any concentration of NH3, the response of the gas sensor prepared using the SnO2@GO@Gr composite film of this embodiment is significantly higher than that of the Gr sensor. For example, for 100ppm NH3, the response of the composite film sensor in this embodiment is 20.22%, which is 7.2 times the response of the Gr sensor (2.80%), 2.05 times the gas-sensitive response (9.86%) in Example 1, and 1.2 times the gas-sensitive response (17.11%) in Example 2. This shows that the SnO2@GO@Gr composite structure nanofilm proposed in the present invention has excellent gas-sensitive properties.
[0077] Example 4
[0078] This embodiment M0 X The preparation method of the composite gas-sensitive membrane of @GO co-supported transferred graphene comprises the following steps
[0079] 1) Weigh a certain amount of the above SnO2 powder and add an appropriate amount of anhydrous ethanol to prepare a SnO2 dispersion with a concentration of 1 mg / ml.
[0080] 2) SnO2@GO transfer graphene
[0081] Weigh 20 mg GO, add 20 ml deionized water, shake well, and disperse by ultrasound for 4 hours to obtain a uniform GO dispersion with a concentration of 1 mg / ml. Take 1 mL GO dispersion, add 1 mL SnO2 dispersion prepared in step 1), and then mix by ultrasound for 20 minutes. The ultrasonic power is set to 350 w to make the nano-MO X The particles are firmly attached to the GO sheet to form a SnO2@GO dispersion. Then the SnO2@GO dispersion is dropped on the grown single-layer copper-based CVD graphene, and the dispersion is spin-coated at 500 rpm for 5 seconds using a spin coater, and dried at 85°C for 200 seconds. The resulting device is cut into 0.5×0.5mm 2 Then, SnO2@GO was placed face up on the surface of 3 mol / L (NH4)2S2O8 solution for 4 hours to etch the copper foil substrate at the bottom of the composite film. When the copper foil substrate was completely etched, the SnO2@GO@Gr composite film was obtained.
[0082] By transferring the SnO2@GO@Gr composite film of this embodiment to an electrode substrate, a gas sensor based on the SnO2@GO@Gr composite film can be obtained.
[0083] like Figure 6 As shown, a large number of SnO2 nanoparticles are attached to the GO surface, forming a supporting layer for the transferred graphene. In addition, compared with Example 3, the surface roughness of the film is further increased.
[0084] like Fig. 9 As shown, it can be seen that the initial resistance value of the gas sensor prepared using the SnO2@GO@Gr composite film of this embodiment is 3944Ω, which is 8.5 times the initial resistance value of the Gr sensor, indicating that SnO2@GO in this embodiment can be used as a support layer for Gr transfer, but the integrity of the Gr film is slightly damaged during the transfer process.
[0085] like Fig.10 As shown, it can be seen that for any concentration of NH3, the response of the gas sensor prepared using the SnO2@GO@Gr composite film of this embodiment is significantly higher than that of the Gr sensor. For example, for 100ppm NH3, the response of the composite film sensor in this embodiment is 16.32%, which is 5.8 times the response of the Gr sensor (2.80%) and 1.7 times the gas-sensitive response (9.86%) in Example 1. However, compared with Examples 2 and 3, the gas-sensitive response in this embodiment has decreased, which is 4.6% lower than the gas-sensitive response (17.11%) in Example 2 and 19.3% lower than the gas-sensitive response (20.22%) in Example 3. It shows that the gas-sensitive performance of the SnO2@GO@Gr composite structure nanofilm proposed in the present invention is affected by the mass ratio of GO and SnO2.
[0086] Example 5
[0087] This embodiment M0 X The preparation method of the composite gas-sensitive membrane of @GO co-supported transferred graphene comprises the following steps
[0088] 1) Weigh a certain amount of the above SnO2 powder and add an appropriate amount of anhydrous ethanol to prepare a SnO2 dispersion with a concentration of 10 mg / ml.
[0089] 2) SnO2@GO transfer graphene
[0090] GO was added to deionized water, shaken thoroughly, and ultrasonically dispersed for 4 hours to obtain a uniform GO dispersion with a concentration of 1 mg / ml. 1 mL of GO dispersion was taken, and 1 mL of SnO2 dispersion prepared in step 1) was added thereto, and then ultrasonically mixed for 10 minutes at a power of 400 W. X The particles are firmly attached to the GO sheet to form a SnO2@GO dispersion. Then the SnO2@GO dispersion is dropped on the grown single-layer copper-based CVD graphene, and the dispersion is spin-coated at 100 rpm for 60 seconds using a spin coater, and dried at 80°C for 300 seconds. The resulting device is cut into 0.5×0.5mm 2Then, SnO2@GO was placed face up on the surface of 1 mol / L (NH4)2S2O8 solution for 5 hours to etch the copper foil substrate at the bottom of the composite film. When the copper foil substrate was completely etched, the SnO2@GO@Gr composite film was obtained.
[0091] By transferring the SnO2@GO@Gr composite film of this embodiment to an electrode substrate, a gas sensor based on the SnO2@GO@Gr composite film can be obtained.
[0092] like Figure 7 As shown, a large number of SnO2 nanoparticles are attached to the GO surface, forming a support layer for the transferred graphene. In addition, the surface roughness of the film is greater than that of Examples 3 and 4, and the SnO2 nanoparticles appear in clusters.
[0093] like Fig. 9 As shown, it can be seen that the initial resistance value of the gas sensor prepared by using the SnO2@GO@Gr composite film of this embodiment is 15336Ω, which is two orders of magnitude higher than the initial resistance value of the Gr sensor. This may be due to the destruction of the integrity of the Gr during the transfer process. Figure 6 and Figure 8 Analysis shows that SnO2@GO in this embodiment can serve as a transfer support layer for Gr, but due to the substantial increase in SnO2 content, the GO wrapping is enhanced, which to a certain extent hinders the combination of GO sheets and single-layer Gr, resulting in severe damage to Gr during the transfer process.
[0094] like Fig.10 As shown, it can be seen that for any concentration of NH3, the response of the gas sensor prepared using the SnO2@GO@Gr composite film of this embodiment is significantly higher than that of the Gr sensor. For example, for 100ppm NH3, the response of the composite film sensor in this embodiment is 15.17%, which is 5.4 times the response of the Gr sensor (2.80%) and 1.5 times the gas-sensitive response (9.86%) in Example 1. However, compared with Example 2, Example 3 and Example 4, the high mass ratio (1:10) in this embodiment reduces the response of the gas-sensitive film, which is 11% lower than the gas-sensitive response (17.11%) in Example 2, 25% lower than the gas-sensitive response (20.22%) in Example 3, and 7% lower than the gas-sensitive response (16.32%) in Example 4. It shows that the gas-sensitive performance of the SnO2@GO@Gr composite structure nanofilm proposed in the present invention is affected by the mass ratio of GO and SnO2.
[0095] Comparative Example 1
[0096] This comparative example MO X The preparation method of the composite gas-sensitive membrane of @GO co-supported transferred graphene comprises the following steps
[0097] 1) GO transfer graphene
[0098] Weigh 20 mg GO, add 20 ml deionized water, shake well, and disperse by ultrasound for 4 hours to obtain a uniform GO dispersion with a concentration of 1 mg / ml. Then drop the SnO2@GO dispersion on the grown single-layer copper-based CVD graphene, spin coat it at 500 rpm for 5 seconds using a gel coater, and dry it at 80°C for 30 seconds. Cut the resulting device into 0.5×0.5 mm 2 Then, the GO surface was placed upward and floated on the surface of 1 mol / L (NH4)2S2O8 solution for 5 hours to etch the copper foil substrate at the bottom of the composite film. When the copper foil substrate was completely etched, the GO@Gr composite film was obtained.
[0099] The GO@Gr composite film of this comparative example is transferred to an electrode substrate to obtain a gas sensor based on the GO@Gr composite film.
[0100] like Figure 8 As shown, GO is tightly compounded on the Gr surface, forming a good supporting layer for transferred graphene.
[0101] like Fig. 9 As shown, it can be seen that the initial resistance values of the two sensors are close, 470Ω and 464Ω, respectively, indicating that GO in this comparative example can serve as a good support layer and fully ensure the integrity of Gr during the transfer process.
[0102] like Fig.10 As shown, it can be seen that for any concentration of NH3, the response of the gas sensor prepared using the GO@Gr composite film in this comparative example is significantly higher than that of the Gr sensor. For example, for 100ppm NH3, the response of the composite film sensor in this embodiment is 8.2%, which is 2.9 times the response of the Gr sensor (2.80%). However, the response of the gas-sensitive film in this comparative example is lower than that of Example 1, Example 2, Example 3, Example 4 and Example 5, which is 83% of the gas-sensitive response (9.86%) in Example 1, 48% of the gas-sensitive response (17.11%) in Example 2, 41% of the gas-sensitive response (20.22%) in Example 3, 50% of the gas-sensitive response (16.32%) in Example 4, and 54% of the gas-sensitive response (15.17%) in Example 5. This comparative example shows that the addition of SnO2 nanoparticles is beneficial to improving the gas-sensitive response of the SnO2@GO@Gr composite sensitive film.
Claims
1. A kind of MO X The composite gas-sensitive membrane of @GO co-supported transferred graphene is characterized in that: The graphene layer includes a MO X @GO layer, the MO X The @GO layer includes graphene oxide sheets and metal oxide nanoparticles attached to the graphene oxide sheets.
2. A MO according to claim 1 X The composite gas-sensitive membrane of @GO co-supported transferred graphene is characterized in that: The diameter of the graphene oxide sheet is 1 μm-100 μm; the particle size of the metal oxide nanoparticles is 5-50 nm; and the mass ratio of the graphene oxide sheet to the metal oxide nanoparticles is 1:(0.1-10).
3. A MO according to claim 1 X The composite gas-sensitive membrane of @GO co-supported transferred graphene is characterized in that: The graphene layer is a single-layer graphene or a few-layer graphene.
4. A MO according to claim 1 X The composite gas-sensitive membrane of @GO co-supported transferred graphene is characterized in that: The metal oxide nanoparticles include at least one of SnO2, ZnO, Co3O4, V2O5, CuO and Fe2O3.
5. A MO according to claim 1 X The composite gas-sensitive membrane of @GO co-supported transferred graphene is characterized in that: The invention also includes a substrate, which is arranged on the graphene layer and is connected to the MO X @The surface opposite to the GO layer.
6. An MO according to any one of claims 1 to 5 X The preparation method of the composite gas-sensitive membrane of @GO co-supported transferred graphene is characterized in that: The process includes the following: The metal oxide nanoparticle dispersion is uniformly dispersed in the graphene oxide dispersion, and then ultrasonic dispersion is performed to make the metal oxide nanoparticles adhere to the graphene oxide sheet to form MO X @GO dispersion; The MO X @GO dispersion is spin-coated on the prepared graphene layer surface to form MO X @GO@Gr composite structure nanofilm, and then dried to obtain the MO X Composite gas-sensitive film of @GO co-supported transferred graphene.
7. A MO according to claim 6 X The preparation method of the composite gas-sensitive membrane of @GO co-supported transferred graphene is characterized in that: The metal oxide nanoparticles are firstly ground and dispersed, and then the ground and dispersed metal oxide nanoparticles are uniformly dispersed in the graphene oxide dispersion.
8. A MO according to claim 6 X The method for preparing a composite gas-sensitive membrane of @GO co-supported transferred graphene is characterized by: The concentration of the metal oxide nanoparticle dispersion is 0.1-10 mg / ml; the concentration of the graphene oxide dispersion is 0.1-10 mg / mL, the power of ultrasonic dispersion is 200-400w, and the time is 10-60 minutes.
9. A MO according to claim 6 X The method for preparing a composite gas-sensitive membrane of @GO co-supported transferred graphene is characterized by: The MO X When the GO dispersion is spin-coated on the surface of the prepared graphene layer, the spin-coating speed is 100-1000 rpm and the spin-coating time is 1-60 seconds; The MO X After the @GO dispersion is spin-coated on the surface of the prepared graphene layer, it is dried at a temperature of 80-100° C. and a drying time of 30-300 seconds.
10. A MO according to claim 6 X The method for preparing a composite gas-sensitive membrane of @GO co-supported transferred graphene is characterized by: The graphene layer is prepared on the surface of the copper foil substrate; The preparation method also includes a process of etching the copper foil substrate: placing the side with the copper foil substrate in an etching solution for etching, removing the copper foil substrate, and then rinsing the remaining part to obtain the MO X @GO co-supported transferred graphene composite gas-sensitive film; The solute of the etching solution is FeCl3 or (NH4)2S2O8, the concentration is 1-10 mol / L, and the etching time is 1-5 hours.