PECOD (Polyethylene Chemical Oxygen Demand) sensor based on tungsten trioxide hydride / titanium dioxide nano array as well as preparation method and application of PECOD sensor

By growing PECOD sensors with hydrogenated tungsten trioxide/titanium dioxide nanoarrays on a conductive substrate, the problems of low COD detection sensitivity and environmental pollution in the prior art are solved, and efficient and environmentally friendly water COD detection is achieved.

CN118914318AActive Publication Date: 2024-11-08SOUTH CHINA AGRICULTURAL UNIVERSITY +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411309596.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-08
Estimated Expiration
2044-09-19

AI Technical Summary

Technical Problem

The prior art has low sensitivity and low accuracy when detecting chemical oxygen demand (COD) in water, and requires the use of toxic and corrosive reagents, resulting in high detection costs and environmental pollution.

Method used

Using a PECOD sensor based on hydrogenated tungsten trioxide/titanium dioxide nanoarray, the hydrogenated tungsten trioxide nanoarray was grown on the conductive substrate by solvent thermal method and high-temperature calcination method, and the photocatalytic activity was enhanced by combining titanium dioxide nanorods by sol-gel method. and spectral absorption range to achieve fast and sensitive COD detection.

Benefits of technology

This method does not require the use of toxic reagents and corrosive reagents, and can quickly and accurately detect COD in water. It is simple to operate and avoids harm to the detector and the environment. It has a wide linear range and a low detection limit.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118914318A_ABST
    Figure CN118914318A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of PECOD sensors, and particularly relates to a PECOD sensor based on a tungsten trioxide hydride / titanium dioxide nano array and a preparation method and application of the PECOD sensor. According to the invention, a layer of titanium dioxide nanorods is loaded on the hydrogenated tungsten trioxide nanoplate film, so that not only can a spectrum in a wider range be absorbed, but also photo-generated e-h < + > separation is promoted under an illumination condition, the photocatalytic activity is higher, and the preparation method is simple. Under the light condition, the PECOD sensor utilizes light and current to photoelectrocatalyze organic matters, can be used for measuring COD in wastewater, does not need to use toxic reagents and corrosive reagents, saves time and reagent cost, and avoids influence on health of detection personnel and secondary pollution to the environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of PECOD sensors, and in particular to a PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray, and a preparation method and application thereof. Background Art

[0002] Chemical oxygen demand (COD) refers to the amount of oxidant required to oxidize oxidizable substances in a water sample under specific conditions. COD is often used as an indicator to measure the amount of organic matter in water. The smaller the COD value, the lighter the water pollution. Traditional methods usually use strong oxidants such as dichromate or permanganate to oxidize and degrade organic matter in water or wastewater to estimate COD. This method not only has the disadvantages of low sensitivity, low accuracy, large sample size, and high cost, but also causes a large amount of toxic reagents (such as HgSO4) and corrosive reagents (such as concentrated H2SO4) to be consumed. Therefore, it is of practical value to find a simple and environmentally friendly COD detection method.

[0003] The photoelectrocatalytic oxidation method can be used to fix the semiconductor photocatalyst on a conductive substrate as a working electrode, and to make a composite electrode with a material having electrocatalytic activity. The composite electrode generates e - -h + , h generated on the electrode surface + and ·OH free radicals oxidize organic matter in solution, while photogenerated e - Through the external circuit to the counter electrode to reduce the oxidized components, due to e - The unidirectional flow of e - and h + The photoelectric device based on photoelectrocatalytic oxidation inherits the advantages of high efficiency and low consumption of photocatalytic technology, rapid sensitivity and easy miniaturization of electrochemical technology, and has good development prospects in the field of detection. However, it is still a difficult problem to develop a simple, cheap and sensitive photoelectrode material for detecting COD value in water by photoelectrocatalytic oxidation. Summary of the invention

[0004] The first object of the present invention is to provide a PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray to solve at least one of the above technical problems.

[0005] The second object of the present invention is to provide a method for preparing a PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray prepared by the above preparation method, so as to solve at least one of the above technical problems.

[0006] The third object of the present invention is to provide an application of the above-mentioned PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray to solve at least one of the above-mentioned technical problems.

[0007] The present invention uses glucose as a detection substrate to replace organic pollutants in wastewater for testing.

[0008] According to a first aspect of the present invention, a PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray is provided. The PECOD sensor of hydrogenated tungsten trioxide / titanium dioxide nanoarray is a layer of titanium dioxide nanorods attached to a hydrogenated tungsten trioxide nanoplate film.

[0009] The PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray of the present invention has a layer of titanium dioxide nanorods attached to the hydrogenated tungsten trioxide nanoplate film, which can not only absorb a wider range of spectra, but also promote photogenerated light under light conditions. - -h + Separation, with higher photocatalytic activity.

[0010] In some embodiments, the hydrogenated WO3 nanoplate film is prepared by the following method: calcining the FTO conductive glass on which the WO3 nanoplates are grown, cooling it down, and then calcining it a second time in an atmosphere of argon-hydrogen mixed gas, and after cooling it down to room temperature, the hydrogenated WO3 nanoplate film can be obtained.

[0011] According to a second aspect of the present invention, a method for preparing a PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray is provided, and the preparation method comprises the following steps:

[0012] S1, ultrasonically treating the fluorine-doped tin oxide conductive glass with acetone, deionized water, and anhydrous ethanol in sequence, then rinsing the fluorine-doped tin oxide conductive glass with deionized water and drying it to obtain a conductive substrate;

[0013] S2. Dissolve sodium tungstate dihydrate in deionized water, slowly add hydrochloric acid solution thereto and stir until a suspension containing light yellow flocculent precipitates is obtained, add ammonium oxalate to the suspension and continue stirring until the suspension becomes clear, add deionized water and stir to obtain a precursor solution;

[0014] S3, transferring the precursor solution to a Teflon lining, placing the conductive substrate against the wall of the Teflon container, placing the conductive surface downward into the precursor solution for hydrothermal reaction, cooling to room temperature, washing the first reaction product with deionized water and drying, and obtaining FTO conductive glass with grown WO3 nanoplates;

[0015] S4, calcining the FTO conductive glass on which the WO3 nanoplates are grown, cooling to room temperature, and then calcining for the second time in an atmosphere of argon-hydrogen mixed gas, cooling to room temperature, to obtain a hydrogenated WO3 nanoplate film;

[0016] S5. Place the hydrogenated WO3 nanoplate film in a mixed solution containing glycerol, anhydrous ethanol and tetrabutyl titanate, treat it at 160-180°C for 10-12h, cool it to room temperature, rinse the second reaction product with deionized water and ethanol for multiple times, dry it naturally and then calcine it to obtain a PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray.

[0017] The present invention grows tungsten trioxide nanoarrays on FTO conductive glass by a solvothermal method, then hydrogenates tungsten trioxide by a high-temperature calcination method, and combines hole titanium dioxide nanorods on hydrogenated tungsten trioxide by a sol-gel method. The preparation method is simple, and the hydrogenated tungsten trioxide is firmly combined with the FTO conductive glass and has good stability. Compared with tungsten trioxide nanoarrays, the present invention improves the lattice degree of tungsten trioxide nanosheets by calcination, and then performs a second calcination treatment in an atmosphere of argon-hydrogen mixed gas to hydrogenate tungsten trioxide and introduce oxygen vacancies that capture electrons, which can not only absorb a wider range of spectra, including visible light and part of ultraviolet light, and enhance the photocatalytic activity of tungsten trioxide, but also promote photogenerated electrons under illumination conditions. - -h + Titanium dioxide acts as a hole blocking material to promote the generation of e - -h + , e - flows through titanium dioxide to the counter electrode, while h + is blocked by titanium dioxide, thus facilitating the photoelectrocatalytic process - -h + Separation, at the same time + Can capture OH in water molecules - , generating free radicals such as ·OH, thereby promoting the photoelectrocatalytic process to oxidize organic matter in water. The photoelectric material prepared by this preparation method has a wide linear range and a low detection limit, can quickly detect COD in water, is simple to operate, and has high sensitivity.

[0018] In some embodiments, in step S1, the ultrasonic time is 20 minutes.

[0019] In some embodiments, in step S2, when sodium tungstate dihydrate is dissolved in deionized water, the amount of sodium tungstate dihydrate used is 0.23-0.46 g, and the amount of deionized water used is 30-60 mL.

[0020] In some embodiments, in step S2, the hydrochloric acid solution can be 10 to 20 mL of a 3 mol / L hydrochloric acid solution, the amount of ammonium oxalate used is 0.2 to 0.4 g, and in the process of adding deionized water to obtain the precursor solution, the amount of deionized water used is 30 to 60 mL.

[0021] In some embodiments, in step S2, hydrochloric acid solution is slowly added thereto and stirred for 5 to 10 minutes, and ammonium oxalate is added to the suspension and stirred for 8 to 12 minutes. 2- The aqueous solution is slowly added with hydrochloric acid solution. Due to the precipitation of tungstic acid, the solution gradually becomes a suspension containing light yellow flocculent precipitates. Subsequently, ammonium oxalate is added to the suspension. Ammonium oxalate serves as a guiding agent to control the growth of tungstic acid crystals, so that the grown tungstic acid crystals have a nanosheet structure.

[0022] In some embodiments, in step S3, the temperature of the hydrothermal reaction is 120-140° C., and the reaction time is 10-11 h; the drying treatment method is to keep the temperature in an oven at 60-70° C. for 1-2 h.

[0023] In some embodiments, in step S4, the treatment method for calcining the FTO conductive glass on which the WO3 nanoplates are grown may be to calcine in a muffle furnace at a calcination temperature of 450-460° C. and a heating rate of 4-5° C. / min for 1-2 hours.

[0024] In some embodiments, in step S4, the second calcination treatment may be performed by calcining in a tubular furnace at a calcination temperature of 250 to 350° C. and a heating rate of 2 to 3° C. / min for 2 to 3 hours.

[0025] In some embodiments, in step S4, the volume ratio of argon to hydrogen in the argon-hydrogen mixed gas may be 92:8. Argon acts as an inert gas to protect, and hydrogen acts as a reducing agent to hydrogenate the FTO conductive glass on which the WO3 nanosheets are grown.

[0026] In some embodiments, in step S5, the volume ratio of glycerol, anhydrous ethanol and tetrabutyl titanate in the mixed solution is (1-10):(20-30):(0.3-0.5).

[0027] In some embodiments, in step S5, the calcination treatment is performed at 400-450° C. for 2-3 hours.

[0028] In step S1 of the present invention, there is no requirement for the size of the conductive substrate, and the conductive substrate only needs to be placed against the wall of the Teflon container.

[0029] In step S3 of the present invention, there is no requirement for the amount of the precursor solution. The conductive substrate can be placed with the conductive surface facing downward into the precursor solution for a hydrothermal reaction.

[0030] According to a third aspect of the present invention, there is provided an application of a PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray prepared by the above-mentioned preparation method, which can be used to detect COD in wastewater.

[0031] The PECOD sensor prepared by the preparation method of the present invention can be used to detect COD in wastewater. The COD value can be estimated through the linear relationship between the net photocurrent value and the theoretical COD. The entire detection process does not require the addition and use of toxic reagents and corrosive reagents, and the operation is simple and the sensitivity is high.

[0032] The beneficial effects of the present invention include:

[0033] (1) The present invention grows hydrogenated tungsten trioxide nanoarrays on a conductive substrate by a solvothermal method and a high-temperature calcination method, and then combines the hollow titanium dioxide nanorods on the hydrogenated tungsten trioxide by a sol-gel method. The preparation method is simple, and the hydrogenated tungsten trioxide is firmly combined with the conductive substrate and has good stability;

[0034] (2) The tungsten trioxide of the present invention is hydrogenated to introduce oxygen vacancies to capture electrons, which can not only absorb a wider range of spectra, including visible light and part of ultraviolet light, but also promote photogenerated electrons under illumination conditions. - -h + Separation; Titanium dioxide acts as a hole blocking material to promote the generation of e - -h + , e - flows through titanium dioxide to the counter electrode, while h + is blocked by titanium dioxide, thus facilitating the photoelectrocatalytic process - -h + Separation, at the same time + Can capture OH in water molecules - , generating free radicals such as ·OH, thereby promoting the photoelectrocatalytic process to oxidize organic matter in water. The photoelectric material prepared by this preparation method has a wide linear range and a low detection limit, and can quickly detect COD in water;

[0035] (3) Compared with the traditional method of detecting COD in wastewater, the PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray of the present invention is used to detect COD in wastewater. The organic matter in water or wastewater is oxidized and degraded by photoelectrocatalytic oxidation. The COD value can be estimated through the linear relationship between the net photocurrent and the theoretical COD. The operation is simple and the sensitivity is high. The whole process does not require the use of toxic and corrosive reagents, which not only saves time and reagent costs, but also avoids the impact on the health of the detection personnel and secondary pollution to the environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The enlarged scanning electron microscope images of the products prepared in different steps of Example 1 of the present invention; Figure 1 (a) is a scanning electron microscope image of the hydrogenated WO3 nanoplate film prepared in steps (1) to (4) of Example 1 of the present invention; Figure 1 (b) is a scanning electron microscopy image of titanium dioxide on the PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray;

[0037] Figure 2 A scanning electron microscope image of a hydrogenated tungsten trioxide / titanium dioxide array on a PECOD sensor based on a hydrogenated tungsten trioxide / titanium dioxide nanoarray prepared in Example 1 of the present invention;

[0038] Figure 3 The linear sweep voltammogram of the PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray prepared in Example 1 of the present invention under light and dark conditions;

[0039] Figure 4 The current response diagram of the PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray prepared in Example 1 of the present invention and solutions with different glucose concentrations;

[0040] Figure 5 The net photocurrent-glucose concentration relationship diagram of the PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray prepared in Example 1 of the present invention and the photoelectrodes prepared in Comparative Examples 1-3 and solutions with different glucose concentrations;

[0041] Figure 6 For the present invention Figure 5 The linear relationship diagram of net photocurrent-theoretical COD obtained by data calculation is shown in Figure 2. DETAILED DESCRIPTION

[0042] The present invention is further described in detail below in conjunction with the accompanying drawings, but the embodiments of the present invention are not limited thereto. The raw materials and reagents involved in the following examples can all be obtained from commercial channels.

[0043] In the following examples, the fluorine-doped tin oxide conductive glass is cut into 2×5 cm 2 of blocky shape.

[0044] Example 1

[0045] This embodiment provides a method for preparing a PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray, comprising the following steps:

[0046] (1) ultrasonically treating the fluorine-doped tin oxide conductive glass with acetone, deionized water, and anhydrous ethanol for 20 minutes each, then rinsing the fluorine-doped tin oxide conductive glass with deionized water and drying it in an oven to obtain a conductive substrate, which is stored for later use;

[0047] (2) 0.23 g of sodium tungstate dihydrate was dissolved in 30 mL of deionized water, 10 mL of 3 mol / L hydrochloric acid solution was slowly added and stirred for a period of time until a suspension containing a light yellow flocculent precipitate was obtained, and then 0.2 g of ammonium oxalate was added to the suspension, and the stirring was continued for 10 min until the suspension became clear, and then 30 mL of deionized water was added and stirred for 10 min to obtain a precursor solution;

[0048] (3) Take 30mL of the precursor solution and transfer it to a Teflon liner with a capacity of 50mL, place the conductive substrate against the wall of the Teflon container, put it into the precursor solution with the conductive surface facing down, and hydrothermally react at 120°C for 10h, cool to room temperature, repeatedly rinse the conductive substrate containing the tungsten trioxide nanoarray several times with deionized water and ethanol, and dry it in a constant temperature oven for 1h to obtain FTO conductive glass with WO3 nanoplates grown;

[0049] (4) The FTO conductive glass on which the WO3 nanoplate was grown was first placed in a muffle furnace at a temperature of 450°C and a heating rate of 5°C / min and calcined for 1 h. After cooling to room temperature, it was transferred to a high-temperature resistant crucible porcelain boat and placed in a tubular furnace containing an argon and hydrogen atmosphere. The second calcination treatment was performed in a tubular furnace at a temperature of 250°C and a heating rate of 2°C / min for 2 h. After cooling to room temperature, a hydrogenated WO3 nanoplate film was obtained.

[0050] (5) The hydrogenated WO3 nanoplate film was placed in a mixed solution containing 5 mL of glycerol, 25 mL of anhydrous ethanol and 300 μL of tetrabutyl titanate, treated at 180 °C for 10 h, cooled to room temperature, and the second reaction product was rinsed multiple times with deionized water and ethanol. After natural drying, it was calcined in a muffle furnace at 400 °C for 3 h to obtain a PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarrays.

[0051] The surface morphology of hydrogenated tungsten trioxide and titanium dioxide on the prepared PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray was observed by scanning electron microscopy. Figure 1 and Figure 2 As shown, Figure 1 (a) is a scanning electron microscope image of the hydrogenated WO3 nanoplate film prepared in steps (1) to (4) of Example 1 of the present invention; Figure 1 (b) is a scanning electron microscope image of titanium dioxide on the PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray prepared in Example 1 of the present invention; Figure 2 This is a scanning electron microscope image of the hydrogenated tungsten trioxide / titanium dioxide array on the PECOD sensor based on the hydrogenated tungsten trioxide / titanium dioxide nanoarray prepared in Example 1 of the present invention. Figure 1 (a) It can be seen that the growth and distribution of hydrogenated tungsten trioxide nanoarrays on the FTO conductive glass are relatively uniform. After step (4), the surface morphology of hydrogenated tungsten trioxide is nanosheet-like. Figure 1 (b) It can be seen that after step (5), titanium dioxide is loaded on hydrogenated tungsten trioxide in the form of nanorods; Figure 2 and Figure 1 By comparison, it can be seen that the titanium dioxide nanorods cover the originally smooth surface of the hydrogenated tungsten trioxide array more evenly, indicating that the hydrogenated tungsten trioxide / titanium dioxide nanoarray was successfully synthesized on the conductive substrate by the sol-gel method.

[0052] Example 2

[0053] This embodiment provides a method for preparing a PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray, comprising the following steps:

[0054] (1) ultrasonically treating the fluorine-doped tin oxide conductive glass with acetone, deionized water, and anhydrous ethanol for 20 minutes each, then rinsing the fluorine-doped tin oxide conductive glass with deionized water and drying it in an oven to obtain a conductive substrate, which is stored for later use;

[0055] (2) 0.46 g of sodium tungstate dihydrate was dissolved in 30 mL of deionized water, 10 mL of 3 mol / L hydrochloric acid solution was slowly added and stirred for a period of time until a suspension containing a light yellow flocculent precipitate was obtained, and then 0.4 g of ammonium oxalate was added to the suspension, and the stirring was continued for 10 min until the suspension became clear, and then 30 mL of deionized water was added and stirred for 10 min to obtain a precursor solution;

[0056] (3) 30 mL of the precursor solution was transferred to a Teflon liner with a capacity of 50 mL, the conductive substrate was placed against the wall of the Teflon container, and the conductive surface was placed downward into the precursor solution, and the reaction was hydrothermally reacted at 120 ° C for 10 h, cooled to room temperature, and the first reaction product was repeatedly rinsed with deionized water and ethanol several times, and dried in a constant temperature oven for 1 h to obtain FTO conductive glass with WO3 nanoplates grown;

[0057] (4) The FTO conductive glass grown with WO3 nanoplates was first placed in a muffle furnace at a temperature of 400°C and a heating rate of 5°C / min for calcination for 1 hour. After the conductive substrate containing the hydrogenated tungsten trioxide nanoarray was cooled to room temperature, the FTO conductive glass grown with WO3 nanoplates was transferred to a high-temperature resistant crucible porcelain boat and placed in a tubular furnace containing an argon and hydrogen atmosphere. The second calcination treatment was performed in the tubular furnace at a temperature of 350°C and a heating rate of 3°C / min for 2 hours. After cooling to room temperature, a hydrogenated WO3 nanoplate film was obtained;

[0058] (5) The hydrogenated WO3 nanoplate film was placed in a mixed solution containing 10 mL of glycerol, 20 mL of anhydrous ethanol and 500 μL of tetrabutyl titanate, treated at 200 °C for 12 h, cooled to room temperature, and the second reaction product was rinsed multiple times with deionized water and ethanol. After natural drying, it was calcined in a muffle furnace at 350 °C for 2 h to obtain a PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarrays.

[0059] Example 3

[0060] This embodiment provides an application of a PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray, which can be used to detect the content of organic pollutants in water, including the following steps:

[0061] (1) preparing a set of standard solutions of detection substrates of different concentrations including blank standard samples, and drop-coating the standard solutions of detection substrates of different concentrations onto the PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray prepared in Example 1 or 2;

[0062] (2) The PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray was used as the working electrode, the platinum sheet was used as the counter electrode, and the Ag / AgCl was used as the reference electrode to form a three-electrode system. The net photocurrent of the substrate was detected under light conditions using the linear sweep voltammetry of the electrochemical workstation in the electrolyte, and a linear relationship diagram of the net photocurrent-concentration was drawn;

[0063] (3) The wastewater is dripped onto the PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray prepared in Example 1 or 2, and the net photocurrent of the wastewater is detected according to step (2), and a linear relationship diagram of the net photocurrent-concentration is drawn. The content of the electrolyzed organic compound is obtained according to the linear relationship diagram, and the COD of the wastewater is indirectly calculated.

[0064] The detection substrate may be an organic substance, and preferably, the detection substrate may be any one of glucose or glutaric acid.

[0065] Comparative Example 1

[0066] This comparative example provides a method for preparing a photoelectrode based on tungsten trioxide / titanium dioxide nanoarrays. The difference from Example 1 is that this comparative example does not include step (4).

[0067] Comparative Example 2

[0068] This comparative example provides a method for preparing a photoelectrode based on hydrogenated tungsten trioxide nanoarrays. The difference from Example 1 is that this comparative example does not include step (5).

[0069] Comparative Example 3

[0070] This comparative example provides a photoelectrode based on tungsten trioxide nanoarrays. The difference from Example 1 is that this comparative example does not include steps (4)-(5).

[0071] Next, the PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray prepared by the preparation method of Example 1 and the photoelectrodes prepared by the preparation methods of Comparative Examples 1-3 were subjected to application tests.

[0072] The present invention uses glucose as a detection substrate to replace organic pollutants in wastewater for application testing, and the electrolyte used is a 0.5 mol / L Na2SO4 solution.

[0073] Experimental Example 1

[0074] In this experiment, the linear sweep voltammetry of the electrochemical workstation was used. The PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray prepared in Example 1 was selected as the working electrode, the platinum sheet was used as the counter electrode, and the Ag / AgCl was used as the reference electrode to form a three-electrode system. The initial potential of the electrochemical workstation was set to 0 V, the termination potential was set to 1.2 V, the scanning speed was set to 0.1 V / s, the sampling interval was set to 0.001 V, the standing time was set to 2 s, and the sensitivity was set to 1×10 -3 A, the current of the PECOD sensor in the electrolyte without glucose was tested under light conditions and dark conditions. The results are shown in Figure 3 As shown. Figure 3It can be seen that the photocurrent density of the PECOD sensor under light conditions is significantly higher than that under dark conditions, indicating that the photocurrent is generated by the photocatalytic reaction of the hydrogenated tungsten trioxide / titanium dioxide nanoarray. Under light conditions, more photogenerated electrons are generated on the surface of the PECOD sensor to participate in the electrochemical reaction.

[0075] Experimental Example 2

[0076] In this experimental example, a three-electrode system was used to test the relationship between the photocurrent and the organic matter concentration of the PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray during the photoelectrocatalytic process of organic matter by chronoamperometry.

[0077] Prepare glucose standard solutions with concentrations of 0.00625mmol / L, 0.125mmol / L, 0.25mmol / L, 0.5mmol / L, 0.75mmol / L, 1mmol / L, 1mmol / L, 1.5mmol / L, 2mmol / L, 2.5mmol / L, and 3mmol / L, and a blank standard sample without glucose;

[0078] The PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray prepared in Example 1 was selected as the working electrode, the platinum sheet was used as the counter electrode, and the Ag / AgCl was used as the reference electrode to form a three-electrode system. The initial potential of the electrochemical workstation was set to 0 V, the termination potential was set to 1.4 V, the scanning speed was set to 0.1 V / s, the sampling interval was set to 0.001 V, the standing time was set to 2 s, and the sensitivity was set to 1×10 -3 A, in the simulated solar radiation (AM1.5G, 300mW / cm 2 ) were used to test the current variation trend of the PECOD sensor and the solutions of glucose with different concentrations including the blank standard in the photoelectrocatalytic process. The results are as follows Figure 4 As shown. Figure 4 It can be seen that the PECOD sensor (H-WO3 / TiO2) generates photocurrent under illumination conditions due to the photocatalytic reaction of hydrogenated tungsten trioxide and titanium dioxide. The current under illumination conditions is significantly higher than that under dark conditions. At the same time, the photocurrent density increases with the increase of glucose concentration in the solution, indicating that glucose participates in the photoelectrocatalytic reaction. When the glucose concentration increases, glucose molecules provide more reaction sites for photogenerated holes, so that photogenerated holes can be consumed more effectively, thereby improving the photoelectrocatalytic efficiency. It also shows that the sensitivity of using PECOD sensors to detect glucose concentration in solution is high. In addition, with the increase of time, the photocurrent density detected at the same glucose concentration remains basically unchanged, indicating that the photocatalytic reaction between PECOD sensors and organic matter is relatively stable within a certain period of time.

[0079] Experimental Example 3

[0080] In this experimental example, a three-electrode system was used to test the photoelectrodes prepared in Example 1 and Comparative Examples 1-3 in photoelectrocatalysis of organic compounds by chronoamperometry.

[0081] Prepare glucose standard solutions with concentrations of 0.00625mmol / L, 0.125mmol / L, 0.25mmol / L, 0.75mmol / L, 1mmol / L, 1mmol / L, 1.5mmol / L, 2mmol / L, 2.5mmol / L and a blank standard sample without glucose respectively;

[0082] The photoelectrodes prepared in Example 1 and Comparative Examples 1-3 were selected as working electrodes, platinum sheets as counter electrodes, and Ag / AgCl as reference electrodes to form a three-electrode system. The initial potential of the electrochemical workstation was set to 0 V, the end potential to 1.2 V, the scanning speed to 0.1 V / s, the sampling interval to 0.001 V, the standing time to 2 s, and the sensitivity to 1×10 -3 A. Test different working electrodes under simulated solar radiation (AM1.5G, 300mW / cm 2 ) under the illumination conditions of the above-mentioned solutions with different concentrations of glucose including the blank standard sample, the current variation trend over time during the photoelectrocatalytic process was analyzed, and the relationship between the net photocurrent of different working electrodes and the glucose concentration was plotted. The results are shown in Figure 5 As shown. Figure 5 It can be seen that compared with the photoelectrodes prepared in Comparative Examples 1-3, the PECOD sensor (H-WO3 / TiO2) based on hydrogenated tungsten trioxide / titanium dioxide nanoarray prepared in Example 1 has the highest net photocurrent when reacting with the same concentration of glucose solution, indicating that the PECOD sensor prepared by the preparation method generates more photogenerated electrons on the surface to participate in the electrochemical reaction under the same lighting conditions, has a higher efficiency of electron transfer, and has a higher efficiency of glucose degradation, and can degrade organic matter to reduce COD in wastewater. At the same time, with the change of glucose concentration, the net photocurrent of the PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray prepared in Example 1 changes to a large extent, indicating that the PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray prepared in Example 1 is highly sensitive to changes in glucose concentration and can be used as a highly sensitive PECOD sensor to detect theoretical COD in wastewater.

[0083] use Figure 5 The photocurrent data of the PECOD sensor photoelectrocatalyzed different concentrations of glucose solutions were plotted to draw a linear relationship between the net photocurrent of the glucose molecule and the theoretical COD, as shown in Figure 6 As shown. Figure 6 It can be seen that when the PECOD sensor detects glucose standard solutions of different concentrations, the net photocurrent (I A ) and theoretical COD(COD Th ) show a high positive correlation.

[0084] According to Fick's law, the molar concentration of organic matter C b With the net current I net The relationship is shown in formula (I),

[0085]

[0086] Since the theoretical COD and C b The calculation formula is:

[0087]

[0088] According to formula (I) and formula (II), we can get net The calculation formula of ThCOD is:

[0089]

[0090] Among them, I net is the net photocurrent generated during the photoelectrocatalytic process (μA), n is the number of electrons transferred when the organic matter is mineralized, A is the area of ​​the working electrode, F is the Faraday constant, D is the organic diffusion coefficient, δ represents the thickness of the Nernst diffusion layer, and C b is the molar concentration of organic matter (mol / L), C m is the mass concentration of organic matter (mg / L), and M is the molar mass of organic matter.

[0091] Because I A The net photocurrent per unit area generated in the photoelectrocatalytic process of the present invention (mA / cm 2 ), COD Th is the theoretical COD (mg / L) of the present invention, satisfying:

[0092] I net =I A ×A×κ, formula (IV)

[0093] COD Th =[ThCOD]×α, formula (V)

[0094] Substituting formula (IV) and formula (V) into formula (III) yields:

[0095]

[0096] Formula (VI) shows that according to Fick's law, the net photocurrent is proportional to the theoretical COD, and the result is Figure 6 Confirm each other.

[0097] Where a and b are the net photocurrent-theoretical COD curves ( Figure 6 ), κ is the slope and intercept of I net with I A α is the unit conversion coefficient between [ThCOD] and the theoretical COD of the present invention.

[0098] Therefore, according to Figure 6 It can be seen that the linear relationship between the net photocurrent and the theoretical COD can be obtained by detecting the net photocurrent in the water through the three-electrode system, and the COD value can be calculated according to the linear relationship. In summary, the PECOD sensor of the present invention can be used as a working electrode, using the three-electrode system to oxidize organic matter in the water body, and record the current change data in detail. The linear relationship between the net photocurrent and the theoretical COD can be used to indirectly calculate the organic matter content in the water body, such as for detecting the COD value in wastewater.

[0099] Therefore, compared with the prior art, the beneficial effects of the present invention are as follows: the PECOD sensor prepared by the present invention is loaded with hydrogenated tungsten trioxide and titanium dioxide, which can not only absorb a wider range of spectra, but also has higher photocatalytic activity. At the same time, the three-electrode system is used to detect the current change through an electrochemical workstation, and the organic matter content in the water body is indirectly calculated through the relationship between the net photocurrent and the theoretical COD in the photoelectric catalytic process. The PECOD sensor can be used for the detection of COD in wastewater.

[0100] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray, characterized in that: A layer of titanium dioxide nanorods is attached to the hydrogenated tungsten trioxide nanoplate film; the hydrogenated WO3 nanoplate film is prepared by the following method: FTO conductive glass grown with WO3 nanoplates is calcined, and after cooling, a second calcination treatment is performed in an atmosphere of argon-hydrogen mixed gas, and after cooling to room temperature, a hydrogenated WO3 nanoplate film can be obtained.

2. The method for preparing the PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray according to claim 1, characterized in that: The preparation method thereof comprises the following steps: S1, ultrasonically treating the fluorine-doped tin oxide conductive glass with acetone, deionized water, and anhydrous ethanol in sequence, then rinsing the fluorine-doped tin oxide conductive glass with deionized water and drying it to obtain a conductive substrate; S2, dissolving sodium tungstate dihydrate in deionized water, slowly adding hydrochloric acid solution thereto and stirring until a suspension is obtained, adding ammonium oxalate to the suspension and continuing to stir until the suspension becomes clear, adding deionized water and stirring to obtain a precursor solution; S3, transferring the precursor solution to a Teflon lining, placing the conductive substrate against the wall of the Teflon container, placing the conductive surface downward into the precursor solution for hydrothermal reaction, cooling to room temperature, washing the first reaction product with deionized water and drying, and obtaining FTO conductive glass with grown WO3 nanoplates; S4, calcining the FTO conductive glass on which the WO3 nanoplates are grown, cooling to room temperature, and then calcining for the second time in an atmosphere of argon-hydrogen mixed gas, and cooling to room temperature to obtain a hydrogenated WO3 nanoplate film; S5. Place the hydrogenated WO3 nanoplate film in a mixed solution containing glycerol, anhydrous ethanol and tetrabutyl titanate, treat it at 160-180°C for 10-12h, cool it to room temperature, rinse the second reaction product with deionized water and ethanol for multiple times, dry it naturally and then calcine it to obtain a PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray.

3. The method for preparing a PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray according to claim 2, characterized in that: In step S2, when sodium tungstate dihydrate is dissolved in deionized water, the amount of sodium tungstate dihydrate used is 0.23-0.46 g, and the amount of deionized water used is 30-60 mL; The hydrochloric acid solution can be 10 to 20 mL of a 3 mol / L hydrochloric acid solution, the amount of ammonium oxalate used is 0.2 to 0.4 g, and the amount of deionized water used in the process of adding deionized water to obtain the precursor solution is 30 to 60 mL.

4. The method for preparing a PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray according to claim 2 or 3, characterized in that: In step S2, hydrochloric acid solution is slowly added thereto and stirred for 5 to 10 minutes, and ammonium oxalate is added to the suspension and stirred for 8 to 12 minutes.

5. The method for preparing a PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray according to claim 2, characterized in that: In step S3, the temperature of the hydrothermal reaction is 120-140° C., and the reaction time is 10-11 h; the drying treatment method is to keep the temperature in an oven at 60-70° C. for 1-2 h.

6. The method for preparing a PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray according to claim 5, characterized in that: In step S4, the treatment method for calcining the FTO conductive glass on which the WO3 nanoplates are grown may be to calcine in a muffle furnace at a temperature of 450-460° C. and a heating rate of 4-5° C. / min for 1-2 hours.

7. The method for preparing a PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray according to claim 6, characterized in that: In step S4, the second calcination treatment may be performed by calcining in a tubular furnace at a temperature of 250 to 350° C. and a heating rate of 2 to 3° C. / min for 2 to 3 hours.

8. The method for preparing a PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray according to claim 2, characterized in that: In step S5, the volume ratio of glycerol, anhydrous ethanol and tetrabutyl titanate in the mixed solution is (1-10):(20-30):(0.3-0.5).

9. The method for preparing a PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray according to claim 2, characterized in that: In step S5, the calcination treatment method is calcination at 400-450° C. for 2-3 hours.

10. Application of the PECOD sensor based on hydrogenated tungsten trioxide / titanium dioxide nanoarray as claimed in claim 1 in detecting the content of organic pollutants in water.

Citation Information

Patent Citations

  • Visible light photoelectrocatalysis based COD (chemical oxygen demand) sensor and preparation method and application thereof

    CN104316581A

  • Preparation method and application research of WO3 nanosheet array film

    CN105384358A

  • Tungsten trioxide / titanium dioxide nano heterojunction thin film and preparation and application thereof

    CN105789352A

  • Layered tungsten trioxide photoelectrode material and preparation method thereof

    CN110054224A

  • Tungsten oxide-based photoelectric catalytic material growing on FTO (Fluorine-doped Tin Oxide) as well as preparation method and application thereof

    CN115672307A