Polarizing film, polarizing plate, and method for producing polarizing film
By using a combination of iodine and titanium compounds in a thin polarizing film, combined with stretching and dyeing treatment, the problem of insufficient durability of polarizing films in the prior art under high temperature and high humidity environments is solved, and high monomer transmittance and Improved durability.
Patent Information
- Application Number
- CN202411141583.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2019-03-13
- Filing Date
- 2020-02-20
- Publication Date
- 2024-11-08
AI Technical Summary
The existing thin polarizing film has insufficient durability in high temperature and high humidity environments, making it difficult to meet the requirements of image display devices for high monomer transmittance and durability.
A polarizing film composed of a polyvinyl alcohol-based resin film containing iodine is used, and a layer of titanium compound is coated on one side. A laminate is formed by stretching and dyeing treatment, and a drying and shrinking treatment is combined to improve durability.
High monomer transmittance and excellent durability in high temperature and high humidity environments are achieved, and the stability and durability of the thin polarizing film are significantly improved.
Smart Images

Figure CN118915221A_ABST
Abstract
Description
[0001] This application is a divisional application of an application with a filing date of February 20, 2020, application number 2020800202971, and invention name of polarizing film, polarizing plate, and method for manufacturing the polarizing film. Technical Field
[0002] The invention relates to a polarizing film, a polarizing plate and a method for manufacturing the polarizing film. Background Art
[0003] In a liquid crystal display device, which is a representative image display device, polarizing films are arranged on both sides of the liquid crystal unit due to its image forming method. As a method for manufacturing a polarizing film, for example, the following method is proposed: a laminate having a resin substrate and a polyvinyl alcohol (PVA) resin layer is stretched, and then dyed to obtain a polarizing film on the resin substrate (for example, Patent Document 1). Using such a method, a thin polarizing film can be obtained, and therefore it has attracted attention as a method that contributes to the thinning of image display devices in recent years. However, thin polarizing films require further improvement in durability under high temperature and high humidity environments.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2001-343521 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] The present invention has been made to solve the above-mentioned conventional technical problems, and its main object is to provide a polarizing film and a polarizing plate having high single-body transmittance and excellent durability in a high-temperature and high-humidity environment, and a method for producing such a polarizing film.
[0009] Solutions for solving problems
[0010] The polarizing film of the present invention is composed of a polyvinyl alcohol-based resin film containing iodine, and has a layer containing a titanium compound on at least one surface.
[0011] In one embodiment, the titanium compound is a water-soluble organic titanium compound. In one embodiment, the water-soluble organic titanium compound is represented by the following formula:
[0012] (HO)2Ti[OCH(CH3)COOR]2
[0013] In the formula, R is a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms.
[0014] In one embodiment, the polarizing film has a thickness of 8 μm or less.
[0015] In one embodiment, the iodine concentration of the polarizing film is 3 wt % or more.
[0016] According to another aspect of the present invention, a polarizing plate is provided, which comprises the polarizing film described above and a protective layer disposed on at least one side of the polarizing film.
[0017] According to another aspect of the present invention, a method for manufacturing the polarizing film is provided. The method comprises the following steps: forming a polyvinyl alcohol-based resin layer on one side of a long thermoplastic resin substrate to form a laminate; stretching and dyeing the laminate to form the polyvinyl alcohol-based resin layer into a polarizing film; and coating at least one surface of the polarizing film with an aqueous solution containing a titanium compound at a concentration of 4 wt % to 50 wt %.
[0018] In one embodiment, the manufacturing method forms a polyvinyl alcohol-based resin layer containing an iodide and a polyvinyl alcohol-based resin on one side of the thermoplastic resin substrate.
[0019] In one embodiment, the manufacturing method comprises the steps of sequentially subjecting the laminate to aerial auxiliary stretching, dyeing, underwater stretching and drying shrinkage treatments, wherein the drying shrinkage treatment is performed by heating while conveying in the length direction, thereby shrinking the laminate in the width direction by more than 2%.
[0020] In one embodiment, the drying and shrinking treatment is performed using a heating roller. In this case, the temperature of the heating roller is, for example, 60°C to 120°C.
[0021] Effects of the Invention
[0022] According to the present invention, a thin polarizing film having high single body transmittance and excellent durability in a high temperature and high humidity environment can be obtained. Such a thin polarizing film can be obtained, for example, by coating an aqueous solution containing a titanium compound at a predetermined concentration on the thin polarizing film. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention.
[0024] Figure 2 This is a schematic diagram showing an example of a drying shrinkage process using a heating roller. DETAILED DESCRIPTION
[0025] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.
[0026] A.Polarizing film
[0027] The polarizing film of the embodiment of the present invention is composed of a polyvinyl alcohol (PVA) resin film containing iodine, and has a layer containing a titanium compound on at least one surface. This layer is typically a coating layer. The coating layer may further contain a water-soluble resin. By providing such a coating layer, the durability of the thin polarizing film in a high temperature and high humidity environment can be improved. It is speculated that this is because the titanium compound acts as a cross-linking agent and cross-links with PVA. Typically, by using such a coating layer, the ΔP described later can be reduced. The effect of the coating layer is more significant in a thin polarizing film. Compared with a thick polarizing film, a thin polarizing film has a higher iodine concentration, the stability of iodine is insufficient, and the humidification durability tends to become insufficient. In this case, the humidification durability can be significantly improved by using a coating layer.
[0028] As the titanium compound, any appropriate titanium compound can be used as long as it can function as a crosslinking agent for the water-soluble resin. Preferably, it is a water-soluble organic titanium compound. The water-soluble organic titanium compound is represented by the following formula (1):
[0029] (HO)2Ti[OCH(CH3)COOR]2···(1)
[0030] In the formula, R is a hydrogen atom, a linear or branched alkyl group having 1 to 5 carbon atoms, preferably a hydrogen atom. Commercially available water-soluble organic titanium compounds may also be used. Specific examples of commercially available products include "ORGATIX TC-315" and "ORGATIX TC-310" manufactured by Matsumoto Fine Chemical Co. Ltd.
[0031] As a water-soluble resin, any appropriate water-soluble resin can be used as long as it can form an aqueous coating layer forming composition (aqueous solution for coating layer). As representative examples, PVA-based resins and water-soluble acrylic resins can be listed. PVA-based resins are preferred. PVA-based resins have excellent adhesion to polarizing films, and further, are easy to form an aqueous solution with excellent operability, and can impart appropriate mechanical strength to the obtained coating layer. As a PVA-based resin, any appropriate PVA-based resin can be used. As a PVA-based resin, for example, the resins described later in the C-1-2 item related to the method for manufacturing polarizing films can be listed.
[0032] The coating layer is formed by applying a coating layer-forming composition (aqueous solution for coating layer) containing a titanium compound, an aqueous medium and a water-soluble resin used as needed to a polarizing film and drying. The concentration of the titanium compound and the water-soluble resin (in the case of existence) in the aqueous solution can be set in consideration of operability (coating properties). The concentration can be adjusted, for example, in such a way that the viscosity of the aqueous solution becomes 1mPa·sec~300mPa·sec. The concentration of the titanium compound in the aqueous solution can be, for example, 4% by weight to 50% by weight. When a water-soluble resin is present, for the ratio of the water-soluble resin to the titanium compound in the aqueous solution (resulting in the coating layer), the titanium compound is, for example, 1 part by weight to 200 parts by weight, preferably 5 parts by weight to 200 parts by weight, and more preferably 10 parts by weight to 100 parts by weight, relative to 100 parts by weight of the water-soluble resin.
[0033] The thickness of the coating layer is preferably 10 nm to 1000 nm, more preferably 50 nm to 800 nm, and further preferably 80 nm to 500 nm. By using the coating layer in the specific thin polarizing film described in this specification, the durability of the polarizing film in a high temperature and high humidity environment can be improved with a much thinner thickness than before. When the coating layer is too thin, the effect brought by the titanium compound sometimes becomes insufficient. When the coating layer is too thick, it is sometimes difficult to dry (as a result, the layer formation itself is difficult) and lacks practicality.
[0034] The general structure of the coating layer is described in, for example, Japanese Patent Application Laid-Open No. 2008-257025, the contents of which are incorporated herein by reference.
[0035] The polarizing film is composed of a PVA-based resin film containing iodine as described above. Preferably, the PVA-based resin constituting the PVA-based resin film (substantially a polarizing film) contains a PVA-based resin modified by acetoacetyl. When it is such a structure, a polarizing film with a desired mechanical strength can be obtained. When the blending amount of the PVA-based resin modified by acetoacetyl is set to 100% by weight as a whole, it is preferably 5% to 20% by weight, and more preferably 8% to 12% by weight. When the blending amount is in such a range, a polarizing film with better mechanical strength can be obtained.
[0036] The thickness of the polarizing film is preferably 8 μm or less, more preferably 7 μm or less, further preferably 5 μm or less, and particularly preferably 3 μm or less. The lower limit of the thickness of the polarizing film may be 1 μm in one embodiment, and may be 2 μm in another embodiment.
[0037] The iodine concentration in the polarizing film is preferably 3% by weight or more, more preferably 4% by weight to 10% by weight, and more preferably 4% by weight to 8% by weight. It should be noted that in this specification, "iodine concentration" refers to the amount of all iodine contained in the polarizing film. More specifically, the iodine in the polarizing film is iodine. - , I2, I3 - 、PVA / I 3- Complex, PVA / I 5- When there are forms such as complexes, the iodine concentration in this specification means the concentration of iodine including all these forms. The iodine concentration can be calculated from the intensity of fluorescent X-rays by fluorescent X-ray analysis and the thickness of the film (polarizing film), for example.
[0038] The monomer transmittance of the polarizing film is preferably 42.0% or more, more preferably 42.5% or more, further preferably 43.5% or more, and particularly preferably 45.0% or more. On the other hand, the monomer transmittance is preferably 48.0% or less, more preferably 46.0% or less. A thin polarizing film with a high monomer transmittance sometimes has reduced durability in a high temperature and high humidity environment. In this case, according to an embodiment of the present invention, even if the thin polarizing film has such a high monomer transmittance, it is possible to achieve excellent durability in a high temperature and high humidity environment. It should be noted that in this specification, when simply recording the monomer transmittance, orthogonal transmittance and polarization degree, it refers to the monomer transmittance, orthogonal transmittance and polarization degree before the durability test. The polarization degree of the polarizing film is preferably 99.95% or more, more preferably 99.99% or more. On the other hand, the polarization degree is preferably 99.998% or less. According to an embodiment of the present invention, it is possible to take into account both high monomer transmittance and high polarization degree in this way, and it is possible to achieve excellent durability in a high temperature and high humidity environment as described later. The above-mentioned single transmittance is typically measured using an ultraviolet visible spectrophotometer and corrected for visual sensitivity. In addition, the single transmittance is a value when the refractive index of one surface of the polarizing plate is converted to 1.50 and the refractive index of the other surface is converted to 1.53. Regarding the above-mentioned polarization degree, it is typically measured using an ultraviolet visible spectrophotometer and corrected for visual sensitivity based on the parallel transmittance Tp and the orthogonal transmittance Tc, and is obtained using the following formula.
[0039] Polarization degree (%) = {(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100
[0040] In the embodiment of the present invention, the change amount ΔP of the polarization degree after a 240-hour durability test at a temperature of 60° C. and a relative humidity of 95% is not less than −0.04%. ΔP is represented by the following formula.
[0041] ΔP=P 240 -P0
[0042] In the above formula, P 240 ρ is the polarization degree after the durability test, and P0 is the polarization degree before the durability test (the polarization degree described above). That is, the polarizing film according to the embodiment of the present invention has a small decrease in polarization degree under a high temperature and high humidity environment.
[0043] The polarizing film can be made using a single resin film or a laminate of two or more layers. As a specific example of a polarizing film obtained using a laminate, a polarizing film obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating the resin substrate can be cited. The polarizing film obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating the resin substrate can be made, for example, in the following manner: a PVA-based resin solution is applied to a resin substrate and dried to form a PVA-based resin layer on the resin substrate, thereby obtaining a laminate of a resin substrate and a PVA-based resin layer; the laminate is stretched and dyed to make the PVA-based resin layer into a polarizing film. In an embodiment of the present invention, an aqueous solution containing a titanium compound at a concentration of 4% to 50% by weight is applied to at least one surface of the polarizing film. Thus, excellent durability in a high temperature and high humidity environment such as described above can be achieved. Preferably, a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin is formed on one side of the resin substrate. Stretching typically includes immersing the laminate in a boric acid aqueous solution and stretching. Furthermore, for stretching, it may also include, as needed, stretching the laminate in the air at a high temperature (e.g., above 95°C) before stretching in the boric acid aqueous solution. Moreover, in the present embodiment, it is preferred that the laminate is provided with a drying shrinkage treatment that shrinks by more than 2% in the width direction by heating while conveying in the length direction. Typically, the manufacturing method of the present embodiment includes the steps of sequentially applying an air auxiliary stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment to the laminate. By introducing auxiliary stretching, the crystallinity of PVA can be improved even when PVA is coated on a thermoplastic resin, and high optical properties can be achieved. In addition, by simultaneously improving the orientation of PVA in advance, the problems of reduction and dissolution of the orientation of PVA can be prevented when immersed in water in the subsequent dyeing process and stretching process, and high optical properties can be achieved. Furthermore, when the PVA-based resin layer is immersed in a liquid, the disorder of the orientation of the polyvinyl alcohol molecules and the reduction of the orientation can be suppressed compared to the case where the PVA-based resin layer does not contain a halide. Thus, the optical properties of the polarizing film obtained by the treatment process of immersing the laminate in a liquid such as dyeing treatment and underwater stretching treatment can be improved. Furthermore, by shrinking the laminate in the width direction by drying shrinkage treatment, the optical properties can be improved. The obtained resin substrate / polarizing film laminate can be used directly (that is, the resin substrate can be used as a protective layer of the polarizing film), or the resin substrate can be peeled off from the resin substrate / polarizing film laminate and any appropriate protective layer that meets the purpose can be stacked on the peeling surface. Details of the method for manufacturing the polarizing film will be described later in Item C.
[0044] B.Polarizing plate
[0045] Figure 1It is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention. The polarizing plate 100 comprises: a polarizing film 10, a first protective layer 20 disposed on one side of the polarizing film 10, and a second protective layer 30 disposed on the other side of the polarizing film 10. The polarizing film 10 is the polarizing film of the present invention described in the above-mentioned item A. One of the first protective layer 20 and the second protective layer 30 may be omitted. In the case where a coating layer is formed on the polarizing film, the protective layer on the coating layer side may be omitted representatively. It should be noted that, as described above, one of the first protective layer and the second protective layer may be a resin substrate used in the manufacture of the above-mentioned polarizing film.
[0046] The first and second protective layers are formed by any appropriate film that can be used as a protective layer of a polarizing film. As a specific example of the material of the main component of the film, cellulose resins such as triacetyl cellulose (TAC), polyester resins, polyvinyl alcohol resins, polycarbonate resins, polyamide resins, polyimide resins, polyethersulfone resins, polysulfone resins, polystyrene resins, polynorbornene resins, polyolefin resins, (meth) acrylic acid resins, acetate resins, etc. can be listed. In addition, thermosetting resins or ultraviolet curing resins such as (meth) acrylic acid resins, carbamate resins, (meth) acrylic acid carbamate resins, epoxy resins, and silicone resins can also be listed. In addition, for example, glassy polymers such as siloxane polymers can also be listed. In addition, the polymer film described in Japanese Patent Publication No. 2001-343529 (WO01 / 37007) can also be used. As the material of the film, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group in the side chain can be used, for example, a resin composition containing an alternating copolymer formed by isobutylene and N-methylmaleimide and an acrylonitrile-styrene copolymer can be cited. The polymer film can be, for example, an extrusion molding of the above resin composition.
[0047] When the polarizing plate 100 is applied to an image display device, the thickness of the protective layer (outer protective layer) disposed on the side opposite to the display panel is typically 300 μm or less, preferably 100 μm or less, more preferably 5 μm to 80 μm, and further preferably 10 μm to 60 μm. It should be noted that, when the surface treatment is performed, the thickness of the outer protective layer is the thickness including the thickness of the surface treatment layer.
[0048] When the polarizing plate 100 is applied to an image display device, the thickness of the protective layer (inner protective layer) disposed on the display panel side is preferably 5 μm to 200 μm, more preferably 10 μm to 100 μm, and further preferably 10 μm to 60 μm. In one embodiment, the inner protective layer is a phase difference layer having any appropriate phase difference value. In this case, the in-plane phase difference Re (550) of the phase difference layer is, for example, 110 nm to 150 nm. "Re (550)" is the in-plane phase difference measured at 23 ° C with light of a wavelength of 550 nm, and is calculated by the formula: Re = (nx-ny) × d. Here, "nx" is the refractive index in the direction where the refractive index in the plane is the largest (ie, the slow axis direction), "ny" is the refractive index in the direction orthogonal to the slow axis in the plane (ie, the fast axis direction), "nz" is the refractive index in the thickness direction, and "d" is the thickness (nm) of the layer (film).
[0049] C. Method for manufacturing polarizing film
[0050] The manufacturing method of a polarizing film of one embodiment of the present invention includes the following steps: applying a PVA-based resin solution on one side of a long thermoplastic resin substrate and drying it to form a PVA-based resin layer, thereby forming a laminate; stretching and dyeing the laminate to form a polarizing film with the PVA-based resin layer; and coating at least one surface of the polarizing film with an aqueous solution containing a titanium compound at a concentration of 4% by weight to 50% by weight (the aqueous solution for the coating layer described in the above item A). By applying the above aqueous solution (representatively by forming a coating layer), a polarizing film with excellent durability in a high temperature and high humidity environment can be achieved. Preferably, the PVA-based resin solution also contains a halide. Preferably, the above manufacturing method includes the steps of sequentially subjecting the laminate to an air auxiliary stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment, wherein the drying shrinkage treatment shrinks the laminate by more than 2% in the width direction by heating while conveying in the length direction. The content of the halide in the PVA-based resin solution (resulting in the PVA-based resin layer) is preferably 5 parts by weight to 20 parts by weight relative to 100 parts by weight of the PVA-based resin. The drying shrinkage treatment is preferably carried out using a heating roller, and the temperature of the heating roller is preferably 60°C to 120°C. The shrinkage rate of the laminate in the width direction caused by the drying shrinkage treatment is preferably 2% or more. According to such a manufacturing method, the polarizing film described in the above-mentioned item A can be obtained. In particular, by preparing a laminate having a PVA-based resin layer containing a halide, making the stretching of the above-mentioned laminate a multi-stage stretching including air auxiliary stretching and underwater stretching, and heating the stretched laminate with a heating roller, a polarizing film having excellent optical properties (representatively, monomer transmittance and unit absorbance) can be obtained.
[0051] C-1. Preparation of laminate
[0052] As a method for producing a laminate of a thermoplastic resin substrate and a PVA-based resin layer, any appropriate method may be adopted. Preferably, a coating solution containing a halide and a PVA-based resin is applied to the surface of the thermoplastic resin substrate and dried to form a PVA-based resin layer on the thermoplastic resin substrate. As described above, the content of the halide in the PVA-based resin layer is preferably 5 to 20 parts by weight relative to 100 parts by weight of the PVA-based resin.
[0053] As a coating method of the coating liquid, any appropriate method can be adopted. For example, roll coating, spin coating, wire rod coating, dip coating, die coating, curtain coating, spray coating, knife coating (comma coating, etc.) and the like can be listed. The coating / drying temperature of the above-mentioned coating liquid is preferably 50° C. or more.
[0054] The thickness of the PVA-based resin layer is preferably 3 μm to 40 μm, more preferably 3 μm to 20 μm.
[0055] Before forming the PVA-based resin layer, the thermoplastic resin substrate may be subjected to a surface treatment (e.g., corona treatment), or an easy-adhesive layer may be formed on the thermoplastic resin substrate. By carrying out such a treatment, the adhesion between the thermoplastic resin substrate and the PVA-based resin layer can be improved.
[0056] C-1-1. Thermoplastic resin substrate
[0057] As the thermoplastic resin substrate, any appropriate thermoplastic resin film may be used. Details of the thermoplastic resin substrate are described in, for example, Japanese Patent Application Laid-Open No. 2012-73580. The entire contents of the publication are incorporated herein by reference.
[0058] C-1-2. Coating liquid
[0059] The coating liquid contains a halide and a PVA-based resin as described above. The coating liquid is typically a solution in which the halide and the PVA-based resin are dissolved in a solvent. As the solvent, for example, water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, various glycols, polyols such as trimethylolpropane, amines such as ethylenediamine and diethylenetriamine can be cited. These can be used alone or in combination of two or more. Among these, water is preferred. The PVA-based resin concentration of the solution is preferably 3 to 20 parts by weight relative to 100 parts by weight of the solvent. At such a resin concentration, a uniform coating film that is tightly attached to the thermoplastic resin substrate can be formed. The content of the halide in the coating liquid is preferably 5 to 20 parts by weight relative to 100 parts by weight of the PVA-based resin.
[0060] The coating liquid may be mixed with additives. As additives, for example, plasticizers, surfactants, etc. may be cited. As plasticizers, for example, polyols such as ethylene glycol and glycerol may be cited. As surfactants, for example, nonionic surfactants may be cited. These may be used for the purpose of further improving the uniformity, dyeability, and stretchability of the obtained PVA-based resin layer.
[0061] As the above-mentioned PVA-based resin, any appropriate resin can be used. For example, polyvinyl alcohol and ethylene-vinyl alcohol copolymer can be listed. Polyvinyl alcohol is obtained by saponifying polyvinyl acetate. Ethylene-vinyl alcohol copolymer is obtained by saponifying ethylene-vinyl acetate copolymer. The saponification degree of PVA-based resin is usually 85 mol% to 100 mol%, preferably 95.0 mol% to 99.95 mol%, and more preferably 99.0 mol% to 99.93 mol%. The saponification degree can be calculated according to JIS K 6726-1994. By using a PVA-based resin with such a saponification degree, a polarizing film with excellent durability can be obtained. When the saponification degree is too high, there is a concern that gelation will occur.
[0062] The average polymerization degree of the PVA-based resin can be appropriately selected depending on the purpose. The average polymerization degree is usually 1000 to 10000, preferably 1200 to 4500, and more preferably 1500 to 4300. The average polymerization degree can be determined in accordance with JIS K 6726-1994.
[0063] As the above-mentioned halide, any appropriate halide can be used. For example, iodide and sodium chloride can be listed. As the iodide, for example, potassium iodide, sodium iodide, and lithium iodide can be listed. Among these, potassium iodide is preferred.
[0064] The amount of the halide in the coating solution is preferably 5 to 20 parts by weight, more preferably 10 to 15 parts by weight, based on 100 parts by weight of the PVA resin. If the amount of the halide exceeds 20 parts by weight, the halide may bleed out, and the resulting polarizing film may become cloudy.
[0065] Generally, by stretching the PVA resin layer, the orientation of the polyvinyl alcohol molecules in the PVA resin will become higher, but if the stretched PVA resin layer is immersed in a liquid containing water, the orientation of the polyvinyl alcohol molecules is sometimes disordered and the orientation is reduced. In particular, when a laminate of a thermoplastic resin and a PVA resin layer is stretched in boric acid water, in order to stabilize the stretching of the thermoplastic resin, when the laminate is stretched in boric acid water at a relatively high temperature, the tendency for the above-mentioned orientation to decrease is significant. For example, the stretching of the PVA film itself in boric acid water is usually carried out at 60°C, while the stretching of the laminate of A-PET (thermoplastic resin substrate) and the PVA resin layer is carried out at a high temperature of about 70°C. In this case, the orientation of the PVA at the initial stage of stretching will decrease in the stage before it rises by stretching in water. In this regard, by preparing a laminate of a PVA-based resin layer containing a halide and a thermoplastic resin substrate, and performing high-temperature stretching (auxiliary stretching) in air before stretching the laminate in boric acid water, the crystallization of the PVA-based resin in the PVA-based resin layer of the laminate after auxiliary stretching can be promoted. As a result, when the PVA-based resin layer is immersed in a liquid, the disorder of the orientation of the polyvinyl alcohol molecules and the reduction of the orientation can be suppressed compared to the case where the PVA-based resin layer does not contain a halide. As a result, the optical properties of the polarizing film obtained by the treatment process of immersing the laminate in a liquid such as dyeing treatment and underwater stretching treatment can be improved.
[0066] C-2. Aerial assisted stretching treatment
[0067] In particular, in order to obtain high optical properties, a two-stage stretching method combining dry stretching (auxiliary stretching) and boric acid water stretching is selected. By introducing auxiliary stretching as in the two-stage stretching, it is possible to suppress the crystallization of the thermoplastic resin substrate while stretching, and it is possible to solve the problem of reduced stretchability due to excessive crystallization of the thermoplastic resin substrate in the subsequent boric acid water stretching, and the laminate is stretched to a higher ratio. Furthermore, in the case of coating a PVA-based resin on a thermoplastic resin substrate, in order to suppress the influence of the glass transition temperature of the thermoplastic resin substrate, it is necessary to lower the coating temperature compared to the case where the PVA-based resin is usually coated on a metal roller, and as a result, the crystallization of the PVA-based resin becomes relatively low and the problem of insufficient optical properties is obtained. In response to this, by introducing auxiliary stretching, even in the case of coating a PVA-based resin on a thermoplastic resin, the crystallinity of the PVA-based resin can be improved, and high optical properties can be achieved. Furthermore, by improving the orientation of the PVA-based resin in advance, it is possible to prevent problems such as a decrease in the orientation and dissolution of the PVA-based resin when immersed in water in the subsequent dyeing and stretching steps, thereby achieving high optical properties.
[0068] The stretching method of aerial auxiliary stretching can be fixed-end stretching (for example, a method of stretching using a tenter stretching machine) or free-end stretching (for example, a method of uniaxially stretching the laminate by passing it between rollers with different circumferential speeds). In order to obtain high optical properties, free-end stretching can be actively adopted. In one embodiment, the aerial stretching process includes a heating roller stretching process, in which the above-mentioned laminate is stretched while being transported along its length direction using the circumferential speed difference between the heating rollers. The aerial stretching process typically includes a regional stretching process and a heating roller stretching process. It should be noted that the order of the regional stretching process and the heating roller stretching process is not limited, and the regional stretching process can be performed first, or the heating roller stretching process can be performed first. The regional stretching process can also be omitted. In one embodiment, the regional stretching process and the heating roller stretching process are performed sequentially. In addition, in another embodiment, in the tenter stretching machine, stretching is performed by holding the end of the film and expanding the distance between the tenters along the flow direction (the expansion of the distance between the tenters is the stretching ratio). At this time, the distance between the tenters in the width direction (perpendicular to the flow direction) is set in an arbitrarily close manner. It is preferred to set the stretch ratio in the flow direction in a manner closer to free-end stretching. In the case of free-end stretching, the shrinkage ratio in the width direction = (1 / stretch ratio) 1 / 2 to calculate.
[0069] The auxiliary stretching in the air can be carried out in one stage or in multiple stages. In the case of multiple stages, the stretching ratio is the product of the stretching ratios of each stage. The stretching direction in the auxiliary stretching in the air is preferably substantially the same as the stretching direction in the underwater stretching.
[0070] The stretching ratio in the air auxiliary stretching is preferably 2.0 to 3.5 times. The maximum stretching ratio when the air auxiliary stretching and the underwater stretching are combined is preferably 5.0 times or more, more preferably 5.5 times or more, and further preferably 6.0 times or more relative to the original length of the laminate. In this specification, the "maximum stretching ratio" refers to the stretching ratio before the laminate is about to break, and refers to the stretching ratio at which the laminate is confirmed to break and is 0.2 lower than this value.
[0071] The stretching temperature of the aerial auxiliary stretching can be set to any appropriate value according to the forming material of the thermoplastic resin substrate, the stretching method, etc. The stretching temperature is preferably above the glass transition temperature (Tg) of the thermoplastic resin substrate, more preferably above the glass transition temperature (Tg) of the thermoplastic resin substrate + 10 ° C, and particularly preferably above Tg + 15 ° C. On the other hand, the upper limit of the stretching temperature is preferably 170 ° C. By stretching at such a temperature, the crystallization of the PVA-based resin can be suppressed from proceeding rapidly, thereby suppressing the adverse conditions caused by the crystallization (for example, hindering the orientation of the PVA-based resin layer caused by stretching).
[0072] C-3. Insolubilization, dyeing and cross-linking
[0073] As needed, an insolubilization treatment is performed after the auxiliary stretching treatment in the air and between the stretching treatment in the water and the dyeing treatment. The above-mentioned insolubilization treatment is typically performed by immersing the PVA-based resin layer in an aqueous solution of boric acid. The above-mentioned dyeing treatment is typically performed by dyeing the PVA-based resin layer with a dichroic substance (typically iodine). As needed, a cross-linking treatment is performed after the dyeing treatment and before the stretching treatment in the water. The above-mentioned cross-linking treatment is typically performed by immersing the PVA-based resin layer in an aqueous solution of boric acid. Details about the insolubilization treatment, the dyeing treatment and the cross-linking treatment are recorded, for example, in Japanese Patent Gazette No. 2012-73580 (mentioned above).
[0074] C-4. Underwater stretching
[0075] The underwater stretching treatment is performed by immersing the laminate in a stretching bath. Through the underwater stretching treatment, the laminate can be stretched at a temperature lower than the glass transition temperature (typically about 80°C) of the thermoplastic resin substrate and the PVA resin layer, and the PVA resin layer can be stretched to a high ratio while suppressing crystallization. As a result, a polarizing film with excellent optical properties can be manufactured.
[0076] The stretching method of the laminate can adopt any appropriate method. Specifically, it can be fixed end stretching or free end stretching (for example, a method of uniaxially stretching the laminate by passing the laminate between rollers with different circumferential speeds). It is preferred to select free end stretching. The stretching of the laminate can be carried out in one stage or in multiple stages. In the case of multiple stages, the stretching ratio (maximum stretching ratio) of the laminate described later is the product of the stretching ratios of each stage.
[0077] The underwater stretching is preferably performed by immersing the laminate in a boric acid aqueous solution (boric acid underwater stretching). By using a boric acid aqueous solution as a stretching bath, the PVA-based resin layer can be given rigidity that can withstand the tension applied during stretching and water resistance that is insoluble in water. Specifically, boric acid generates tetrahydroxyborate anions in an aqueous solution and cross-links with the PVA-based resin through hydrogen bonds. As a result, the PVA-based resin layer can be given rigidity and water resistance so that it can be stretched well, and a polarizing film with excellent optical properties can be manufactured.
[0078] The above-mentioned boric acid aqueous solution is preferably obtained by dissolving boric acid and / or a borate in water as a solvent. The boric acid concentration is preferably 1 to 10 parts by weight, more preferably 2.5 to 6 parts by weight, and particularly preferably 3 to 5 parts by weight relative to 100 parts by weight of water. By setting the boric acid concentration to 1 part by weight or more, the dissolution of the PVA-based resin layer can be effectively suppressed, and a polarizing film with higher characteristics can be manufactured. It should be noted that an aqueous solution obtained by dissolving a boron compound such as borax, glyoxal, glutaraldehyde, etc. in a solvent other than boric acid or a borate can also be used.
[0079] It is preferred to mix an iodide in the stretching bath (boric acid aqueous solution). By mixing an iodide, the dissolution of iodine adsorbed on the PVA-based resin layer can be suppressed. Specific examples of iodide are as described above. The concentration of iodide is preferably 0.05 to 15 parts by weight, more preferably 0.5 to 8 parts by weight relative to 100 parts by weight of water.
[0080] The stretching temperature (liquid temperature of the stretching bath) is preferably 40°C to 85°C, more preferably 60°C to 75°C. At such a temperature, it is possible to stretch to a high ratio while suppressing the dissolution of the PVA-based resin layer. Specifically, as described above, from the perspective of the relationship with the formation of the PVA-based resin layer, the glass transition temperature (Tg) of the thermoplastic resin substrate is preferably above 60°C. In this case, if the stretching temperature is lower than 40°C, there is a concern that stretching cannot be performed well even if the plasticization of the thermoplastic resin substrate brought about by water is considered. On the other hand, the higher the temperature of the stretching bath, the higher the solubility of the PVA-based resin layer becomes, and there is a concern that excellent optical properties cannot be obtained. The immersion time of the laminate in the stretching bath is preferably 15 seconds to 5 minutes.
[0081] The stretching ratio based on underwater stretching is preferably 1.5 times or more, more preferably 3.0 times or more. The total stretching ratio of the laminate is preferably 5.0 times or more, more preferably 5.5 times or more relative to the original length of the laminate. By achieving such a high stretching ratio, a polarizing film with extremely excellent optical properties can be manufactured. Such a high stretching ratio can be achieved by adopting an underwater stretching method (boric acid underwater stretching).
[0082] C-5. Drying shrinkage treatment
[0083] The above-mentioned drying shrinkage treatment can be carried out by a regional heating method that is carried out by heating the entire region, or by heating the conveying roller (using a so-called heating roller) (heating roller drying method). It is preferred to use both of these. By using a heating roller for drying, the heating curling of the laminate can be efficiently suppressed to manufacture a polarizing film with excellent appearance. Specifically, by drying the laminate along the heating roller, the crystallization of the above-mentioned thermoplastic resin substrate can be efficiently promoted to increase the crystallinity, and even at a lower drying temperature, the crystallinity of the thermoplastic resin substrate can be well increased. As a result, the rigidity of the thermoplastic resin substrate increases, thereby becoming a state that can withstand the shrinkage of the PVA-based resin layer caused by drying, and curling is suppressed. In addition, by using a heating roller, the laminate can be dried while maintaining a flat state, so that not only curling but also wrinkles can be suppressed. At this time, the laminate is shrunk in the width direction by the drying shrinkage treatment, and the optical properties can be improved. This is because the orientation of PVA and PVA / iodine complex can be effectively improved. The shrinkage rate of the laminate in the width direction due to the drying shrinkage treatment is preferably 1% to 10%, more preferably 2% to 8%, and particularly preferably 4% to 6%.
[0084] Figure 2 Schematic diagram showing an example of drying shrinkage treatment. In the drying shrinkage treatment, the laminate 200 is dried while being transported by the transport rollers R1 to R6 and the guide rollers G1 to G4 heated to a predetermined temperature. In the example shown in the figure, the transport rollers R1 to R6 are arranged in a manner to alternately and continuously heat the surface of the PVA resin layer and the surface of the thermoplastic resin substrate, but, for example, the transport rollers R1 to R6 may be arranged in a manner to continuously heat only one surface of the laminate 200 (for example, the surface of the thermoplastic resin substrate).
[0085] The drying conditions can be controlled by adjusting the heating temperature of the conveying roller (the temperature of the heating roller), the number of heating rollers, the contact time with the heating roller, etc. The temperature of the heating roller is preferably 60°C to 120°C, more preferably 65°C to 100°C, and particularly preferably 70°C to 80°C. It is possible to produce an optical laminate that can well increase the crystallinity of the thermoplastic resin, thereby well suppressing curling, and has extremely excellent durability. It should be noted that the temperature of the heating roller can be measured by a contact thermometer. Six conveying rollers are provided in the example shown in the figure, but there is no particular limitation as long as there are multiple conveying rollers. Conveying rollers are usually provided in 2 to 40 numbers, preferably 4 to 30 numbers. The contact time (total contact time) between the laminate and the heating roller is preferably 1 second to 300 seconds, more preferably 1 to 20 seconds, and more preferably 1 to 10 seconds.
[0086] The heating roller can be set in a heating furnace (such as an oven) or in a normal production line (under room temperature environment). It is preferably set in a heating furnace equipped with an air supply unit. By combining the drying based on the heating roller and the hot air drying, the rapid temperature change between the heating rollers can be suppressed, and the shrinkage in the width direction can be easily controlled. The temperature of the hot air drying is preferably 30°C to 100°C. In addition, the hot air drying time is preferably 1 second to 300 seconds. The wind speed of the hot air is preferably about 10m / s to 30m / s. It should be noted that the wind speed is the wind speed in the heating furnace and can be measured by a mini blade type digital anemometer.
[0087] C-6. Other treatments
[0088] It is preferred that a cleaning treatment be performed after the underwater stretching treatment and before the drying shrinkage treatment. The cleaning treatment is typically performed by immersing the PVA-based resin layer in an aqueous potassium iodide solution.
[0089] C-7. Formation of coating layer
[0090] By operating as above, a laminate (polarizing plate) of a thermoplastic resin substrate and a polarizing film can be obtained. In an embodiment of the present invention, an aqueous solution containing a titanium compound at a concentration of 4% by weight to 50% by weight (the aqueous solution for the coating layer described in the above-mentioned item A) is applied to at least one surface of the polarizing film. In one embodiment, the aqueous solution is applied to the surface of the polarizing film of the laminate. As a result, a laminate (polarizing plate) of a thermoplastic resin substrate / polarizing film / coating layer can be obtained. In this case, typically, the thermoplastic resin substrate can be used directly as a protective layer of the polarizing film. In another embodiment, a resin film (forming a protective layer) is attached to the surface of the polarizing film of the laminate to produce a laminate of a protective layer / polarizing film / thermoplastic resin substrate, and the thermoplastic resin substrate is peeled off from the laminate to produce a laminate (polarizing plate) of a protective layer / polarizing film. The aqueous solution is applied to the surface of the polarizing film of the obtained polarizing plate. As a result, a laminate (polarizing plate) of a protective layer / polarizing film / coating layer can be obtained.
[0091] As a coating method for the aqueous solution, any appropriate method can be adopted. As a specific example, the method described in Item C-1 as a coating method for a coating liquid for forming a PVA-based resin layer (polarizing film) can be cited. The coated aqueous solution is dried to form a coating layer. The drying temperature is, for example, 40°C to 100°C, and the drying time is, for example, 1 minute to 20 minutes.
[0092] Example
[0093] The present invention is described in detail below by way of examples, but the present invention is not limited to these examples. The measuring methods of various properties are as follows. It should be noted that, unless otherwise specified, the "parts" and "%" in the examples and comparative examples are by weight.
[0094] (1) Thickness
[0095] The polarizing plates (protective layer / polarizing film / coating layer) of the examples and comparative examples were cut, and the cross-section of the polarizing plates was observed using a scanning electron microscope ("JSM7100F" manufactured by JEOL Ltd.) to measure the thickness of the coating layer. The thickness of the polarizing film was measured using an interference film thickness meter ("MCPD-3000" manufactured by Otsuka Electronics Co., Ltd.).
[0096] (2) Single-body transmittance, orthogonal transmittance, and polarization degree
[0097] For the polarizing plates (protective layer / polarizing film / coating layer) of the embodiments and comparative examples, the single transmittance Ts, parallel transmittance Tp, and orthogonal transmittance Tc measured using an ultraviolet visible spectrophotometer (LPF200 manufactured by Otsuka Electronics Co., Ltd.) are set as Ts, Tp, and Tc of the polarizing film, respectively. These Ts, Tp, and Tc are Y values measured using a 2-degree field of view (C light source) of JIS Z8701 and corrected for visual sensitivity. The polarization degree is calculated using the following formula from the obtained Tp and Tc.
[0098] Polarization degree (%) = {(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100
[0099] (3) Optical durability
[0100] Glass (alkali-free glass) with alkali components removed was bonded to the polarizing film side of the polarizing plate of the embodiment and the comparative example with the aid of an adhesive as a test sample. The test sample was subjected to a durability test for 240 hours at a temperature of 60°C and a relative humidity of 95%. The optical properties before and after the durability test were measured using the spectrophotometer described in (2) above, and ΔP was calculated using the following formula.
[0101] ΔP=P 240 -P0
[0102] In the above formula, P 240 is the polarization degree after the durability test, and P0 is the polarization degree before the durability test.
[0103] [Example 1-1]
[0104] As the thermoplastic resin substrate, a long amorphous polyethylene terephthalate copolymer film (thickness: 100 μm) having a Tg of about 75° C. was used. One surface of the resin substrate was subjected to a corona treatment.
[0105] 13 parts by weight of potassium iodide was added to 100 parts by weight of a PVA-based resin prepared by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., trade name "GOHSEFIMER Z410") in a ratio of 9:1 to prepare a PVA aqueous solution (coating solution).
[0106] The PVA aqueous solution was applied to the corona-treated surface of the resin substrate and dried at 60° C. to form a 13 μm-thick PVA-based resin layer, thereby producing a laminate.
[0107] The obtained laminate was uniaxially stretched to 2.4 times at the free end in the longitudinal direction (length direction) between rolls having different peripheral speeds in an oven at 130° C. (in-air auxiliary stretching treatment).
[0108] Next, the laminate was immersed in an insolubilization bath (boric acid aqueous solution prepared by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilization treatment).
[0109] Next, the film was immersed in a dyeing bath (an iodine aqueous solution obtained by mixing iodine and potassium iodide at a weight ratio of 1:7 per 100 parts by weight of water) at a liquid temperature of 30° C. for 60 seconds (dyeing treatment) at a concentration adjusted so that the single body transmittance (Ts) of the final polarizing film was 43.8%.
[0110] Next, the sample was immersed in a crosslinking bath (boric acid aqueous solution prepared by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment).
[0111] Thereafter, the laminate was immersed in an aqueous boric acid solution (boric acid concentration: 4.0 wt %, potassium iodide concentration: 5.0 wt %) at a liquid temperature of 70°C and uniaxially stretched in the longitudinal direction (length direction) between rollers with different peripheral speeds to a total stretching ratio of 5.5 times (underwater stretching treatment).
[0112] Thereafter, the laminate was immersed in a cleaning bath (an aqueous solution prepared by mixing 4 parts by weight of potassium iodide with respect to 100 parts by weight of water) at a liquid temperature of 20° C. (cleaning treatment).
[0113] Thereafter, the laminate was brought into contact with a SUS heating roll having a surface temperature of 75° C. for about 2 seconds while being dried in an oven maintained at 90° C. (drying shrinkage treatment). The shrinkage rate in the width direction of the laminate due to the drying shrinkage treatment was 2%.
[0114] Thus, a polarizing film with a thickness of 5.0 μm was formed on the resin substrate. A cycloolefin film (manufactured by ZEON, product name "G-Film") as a protective layer (protective film) was bonded to the surface of the polarizing film using a UV curable adhesive (thickness 1.0 μm), and then the resin substrate was peeled off to obtain a polarizing plate having a protective layer / polarizing film structure.
[0115] The surface of the polarizing film of the obtained polarizing plate is coated with an aqueous solution for coating layer. The aqueous solution contains 4 wt% of a titanium compound (manufactured by Matsumoto Pharmaceutical Industry Co., Ltd., product name "ORGATIX TC-315"). The coating film of the aqueous solution is dried at 60° C. for 5 minutes to form a coating layer with a thickness of 100 nm, thereby obtaining a polarizing plate having a structure of protective layer / polarizing film / coating layer.
[0116] Table 1 shows ΔP of the obtained polarizing plate (substantially, polarizing film).
[0117] [Example 1-2]
[0118] A polarizing plate was produced in the same manner as in Example 1-1 except that the concentration of the titanium compound in the aqueous coating layer solution was 44% by weight.
[0119] [Example 2]
[0120] A polarizing plate was produced in the same manner as in Example 1-1 except that the single-body transmittance was set to 45%. Table 1 shows ΔP of the obtained polarizing plate (substantially, a polarizing film).
[0121] [Comparative Example 1]
[0122] A polarizing plate was produced in the same manner as in Example 1-1 except that the coating layer was not formed. ΔP is shown in Table 1 for the obtained polarizing plate (substantially, a polarizing film).
[0123] [Comparative Example 2]
[0124] A polarizing plate was produced in the same manner as in Example 2 except that the coating layer was not formed. Table 1 shows ΔP of the obtained polarizing plate (substantially, a polarizing film).
[0125] [Table 1]
[0126]
[0127] As can be seen from Table 1, the polarizing films of Examples of the present invention have excellent durability in a high-temperature and high-humidity environment.
[0128] Industrial Applicability
[0129] The polarizing film and polarizing plate of the present invention are suitable for use in liquid crystal display devices.
[0130] Description of Reference Numerals
[0131] 10 polarizing film
[0132] 20 1st protection layer
[0133] 30 Second protection layer
[0134] 100 polarizing plate
Claims
1. A polarizing plate, comprising: A polarizing film composed of a polyvinyl alcohol-based resin film containing iodine, A coating layer including a titanium compound is formed on one surface of the polarizing film, a protective layer disposed on the surface of the polarizing film on which the coating layer is not formed, The coating layer has no adhesive function and has a thickness of 10 nm to 800 nm.
2. The polarizing plate according to claim 1, wherein The titanium compound is a water-soluble organic titanium compound.
3. The polarizing plate according to claim 2, wherein: The water-soluble organic titanium compound is represented by the following formula: (HO)2Ti[OCH(CH3)COOR]2 In the formula, R is a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms. 4 . The polarizing plate according to claim 1 , wherein the polarizing film has a thickness of 8 μm or less and an iodine concentration of 3% by weight or more.
5. The polarizing plate according to any one of claims 1 to 4, wherein the polarizing film further comprises iodide or sodium chloride. The content of the iodide or sodium chloride in the polarizing film is 5 to 20 parts by weight based on 100 parts by weight of the polyvinyl alcohol-based resin.
6. A manufacturing method, which is the manufacturing method of the polarizing plate according to any one of claims 1 to 5, comprising the following steps: A polyvinyl alcohol-based resin layer containing an iodide and a polyvinyl alcohol-based resin is formed on one side of a long thermoplastic resin substrate to prepare a laminate; The laminate is subjected to an aerial auxiliary stretching treatment, a dyeing treatment, an underwater stretching treatment and a drying shrinkage treatment in sequence, thereby forming the polyvinyl alcohol resin layer into a polarizing film, wherein the drying shrinkage treatment is performed while being transported in the length direction and heated, thereby shrinking the layer in the width direction by more than 2%; forming a coating layer by coating an aqueous solution containing a titanium compound at a concentration of 4 wt % to 50 wt % on one surface of the polarizing film and drying the solution; and A protective layer is laminated on the surface of the polarizing film on which the coating layer is not formed.
7. The manufacturing method according to claim 6, wherein: The drying shrinkage treatment is performed using a heating roller.
8. The manufacturing method according to claim 7, wherein: The temperature of the heating roller is 60°C to 120°C.
Citation Information
Patent Citations
Polariser and polarising plate including same
CN105992961A
Method for manufacturing polariser, and polariser and polarising plate manufactured using same
CN106716194A
Curing type adhesive composition for polarizing film and manufacturing method therefor, polarizing film and manufacturing method therefor, optical film and image display device
CN108027471A
Polarizing plate, optical member provided with the same and liquid crystal display device
JP2008257025A
Polarizing film, polarizing plate, and method for producing polarizing film
JP6409142B1