Photosensitive resin with excellent adhesion property and preparation method thereof
By optimizing the formulation and polymerization reaction steps of the photosensitive resin, combined with silane-modified inorganic filler, the problem of insufficient mechanical properties and stability after curing of the photosensitive resin is solved, and rapid curing, good adhesion and tensile performance are achieved, which is suitable for electronic devices long-term application.
Patent Information
- Application Number
- CN202410958669.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing photosensitive resins are insufficient in mechanical properties and stability after curing, which affects their long-term application in electronic devices. Especially when alkali-soluble polyimide resins form films, they are prone to cracks, which affects their development and film adhesion. Adhesive.
Using a photosensitive resin formula containing a photosensitive resin precursor, a crosslinking agent, a photoinitiator, a polymerization inhibitor, a silane coupling agent and a silane modified inorganic filler, the curing rate of the resin is increased by optimizing the polymerization reaction step and material ratio. , adhesion and tensile properties, while reducing water absorption, enhancing chemical stability and cross-linking density.
The rapid curing, good adhesion and tensile properties of the photosensitive resin are achieved, and the film retention rate of the developing film is not reduced, which significantly improves its storage stability and mechanical properties in electronic devices, making it suitable for long-term applications.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of photosensitive resin preparation, and particularly relates to a photosensitive resin with excellent adhesion performance and a preparation method thereof. Background Art
[0002] Most photosensitive resins are polymer materials formed by the polymerization of monomers such as epoxy, nitroso, acrylic or alkyd under the action of light. They need to be heated and cured. They are generally used in 3D printing, photolithography and other fields, and are mostly used for rapid prototyping of products. Currently, the most common photosensitive resin materials are resin compositions such as photosensitive polyimide, polybenzoxazole, phenolic resin, etc., which have excellent properties. However, with the high integration of semiconductors and display devices, the mechanical properties and stability of commonly used photosensitive resins are insufficient.
[0003] Polyimide refers to a type of aromatic heterocyclic polymer containing an imide ring in the repeating unit of the molecular chain. Its special molecular structure gives it excellent heat resistance and mechanical properties, and it is one of the high-performance polymer materials that are indispensable to the three major industries of "information, energy, and materials". The curing performance of polyimide and its adhesion to the substrate are obviously the key factors affecting its application.
[0004] Patent CN115576171A discloses a negative photosensitive resin composition and a method for preparing a cured pattern. A double cross-linking agent and a double reactive diluent are used in combination. The prepared photosensitive resin composition can obtain a higher development retention rate at low energy during exposure when the cross-linking agent and the reactive diluent are used in combination. The cured film has good adhesion and tensile properties. However, the alkali-soluble polyimide resin film is prone to cracks. Patent CN 110515269A discloses a photosensitive resin composition and a preparation method thereof, a polymer film and a copper-clad laminate. The soft long-chain diamine monomer improves the alkali resistance, heat resistance and flexibility of the polymer film. However, it will have a certain impact on the mechanical properties of the photosensitive resin cured film.
[0005] In view of this, it is particularly important to invent a photosensitive resin with excellent adhesion and stable curing performance without affecting the development retention rate of its cured film. Summary of the invention
[0006] In view of the defects of the prior art, the purpose of the present invention is to provide a photosensitive resin with a faster curing rate, the cured film has good adhesion and tensile properties, and does not affect the development retention rate of the cured film, and is suitable for long-term stable application in electronic devices.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0008] In one aspect, the present invention provides a photosensitive resin having excellent adhesion properties, wherein the photosensitive resin comprises the following raw materials in parts by weight: 10 to 70 parts of a photosensitive resin precursor, 2 to 50 parts of a crosslinking agent, 0.01 to 50 parts of a photoinitiator, 0.01 to 5 parts of a polymerization inhibitor, 0.01 to 5 parts of a silane coupling agent, 20 to 80 parts of an organic solvent 1, 50 to 70 parts of an inorganic filler, 20 to 100 parts of a solvent 1, and 50 to 200 parts of a solvent 2;
[0009] Wherein, the inorganic filler is a silane-modified inorganic filler.
[0010] Preferably, the preparation steps of the photosensitive resin precursor are as follows:
[0011] (1) in a reactor, acrylic acid, acrylic acid ester monomer, and acrylic acid hydroxyl monomer are copolymerized in an organic solvent 2, an initiator and a dispersant are added, and the mixture is reacted at 50 to 70° C. for 4 to 6 hours to obtain an acrylic acid ester polymer;
[0012] (2) firstly adding a first weight portion of an organic solvent 2, a polymerization inhibitor and a catalyst 1 into a reactor, then adding the acrylic ester polymer and the benzene ring-containing ketone compound into the reactor and mixing them, reacting at 0 to 30° C. for 6 to 10 hours to obtain an intermediate 1;
[0013] (3) Adding a second weight portion of organic solvent 2 and catalyst 2 into the reactor, mixing the intermediate 1 with the dianhydride and stirring, and reacting at room temperature for 4 to 10 hours to obtain intermediate 2.
[0014] (4) adding organic solvent 3, intermediate 2, catalyst 3 and acyl chloride reagent to the reactor in sequence, reacting at 0-12° C. for 1-5 h, and reacting at 22-26° C. for 2-8 h to obtain intermediate 3;
[0015] (5) Add diamine and the third part by weight of organic solvent 2 into the reactor and stir evenly, then add intermediate 3 and molecular weight regulator and mix, stir and react at room temperature for 10 to 16 hours, then add dehydrating agent and catalyst 4, react at 0 to 25° C. for 2 to 6 hours to obtain a photosensitive resin precursor.
[0016] Preferably, in the step of preparing the photosensitive resin precursor, the organic solvent 2 is propylene glycol methyl ether acetate, and the organic solvent 3 is dichloromethane.
[0017] Further preferably, the amount of organic solvent 2 added in step (1) is 1.5 to 2 times the total mass of acrylic acid monomer and acrylic ester monomer, the amount of organic solvent 2 added in step (2) is 1.5 to 2 times the total mass of acrylic ester polymer and benzene ring-containing ketone compound, the amount of organic solvent 2 added in step (3) is 2 to 2.5 times the total mass of intermediate 1 and dianhydride, the amount of organic solvent 3 added in step (4) is 3 to 6 times the total mass of intermediate 2 and acyl chloride reagent, and the amount of organic solvent 2 added in step (5) is 2 to 2.5 times the mass of diamine.
[0018] Preferably, in step (1), the molar ratio of the acrylic acid ester monomer to the acrylic acid hydroxyl monomer is (1.2-1.8):1.
[0019] Preferably, the amount of acrylic acid monomer added in step (1) is 1 to 1.2% of the total mass of acrylic acid ester monomer and acrylic acid hydroxyl monomer.
[0020] Preferably, the amount of the initiator added in step (1) is 0.5-1.5% of the total mass of the acrylic acid monomer, the acrylic ester monomer and the acrylic hydroxyl monomer.
[0021] Preferably, the amount of the dispersant added in step (1) is 10 to 40% of the total mass of the acrylic acid monomer, the acrylic ester monomer and the acrylic hydroxyl monomer.
[0022] Preferably, in step (1), the acrylic acid monomer is acrylic acid, the acrylic acid ester monomer is methyl methacrylate, the acrylic acid hydroxyl monomer is hydroxyethyl methacrylate, the initiator is azobisisobutyronitrile, and the dispersant is an inorganic dispersant.
[0023] More preferably, the inorganic dispersant is basic magnesium carbonate.
[0024] The applicant regulates the weight average molecular weight of the acrylate polymer through the preferred steps, so that it maintains a certain chain length and density distribution when used as a part of the main chain of the photosensitive resin precursor, reduces water adsorption, and assists in reducing the water absorption of the photosensitive resin.
[0025] Preferably, in step (2), the molar ratio of the acrylic acid ester polymer to the benzene ring-containing ketone compound is 1:(1-1.2).
[0026] Further preferably, in step (2), the amount of the polymerization inhibitor added is 0.01-0.1% of the total mass of the acrylate polymer and the ketone compound containing a benzene ring, and the amount of the catalyst 1 added is 0.1-1% of the total mass of the acrylate polymer and the ketone compound containing a benzene ring.
[0027] More preferably, in step (2), the inhibitor is p-methoxyphenol, the catalyst 1 is tetraethylammonium bromide, and the benzene ring-containing ketone compound is a benzene ring-containing ethyl ketone compound.
[0028] Preferably, the benzene ring-containing acetone compound is at least one of acetophenone, p-methylacetophenone, p-methoxyacetophenone, p-N,N-dimethylaminoacetophenone and acetonaphthone.
[0029] Preferably, in step (3), the molar ratio of the intermediate 1 to the dianhydride is 1:(1.2-1.8).
[0030] Preferably, the dianhydride in step (3) is at least one of pyromellitic dianhydride and hexafluorodianhydride.
[0031] Preferably, the amount of catalyst 2 added in step (3) is 0.1 to 2.5% of the total mass of the intermediate 1 and the dianhydride.
[0032] More preferably, the catalyst 2 is at least one of sulfuric acid and phosphoric acid.
[0033] Preferably, in step (4), the molar ratio of the intermediate 2 to the acyl chloride reagent is 1:(2-2.2).
[0034] Preferably, the acyl chloride reagent in step (4) is benzoyl chloride.
[0035] Preferably, in step (4), the catalyst 3 is N,N-dimethylformamide.
[0036] More preferably, the mass ratio of the catalyst 3 to the intermediate 2 is 0.05 mL: (250-300) g.
[0037] Preferably, in step (5), the molar ratio of the intermediate 3, the diamine and the molecular weight regulator is 1:(0.8-1.1):(0.01-0.5).
[0038] Preferably, the diamine in step (5) is at least one of p-phenylenediamine and diaminodiphenylmethane.
[0039] Preferably, the molecular weight regulator in step (5) is at least one of phthalic anhydride, hydrogenated phthalic anhydride and aniline.
[0040] Preferably, the dehydrating agent in step (5) is at least one of acetic anhydride and trifluoroacetic anhydride, and the amount added is 1 to 3% of the mass of the diamine.
[0041] Preferably, in step (5), the catalyst 4 is at least one of pyridine and trimethylpyridine.
[0042] Further preferably, the added amount of the catalyst 4 is 1-2% of the mass of the diamine.
[0043] The main chain of the photosensitive resin precursor is an aromatic ring structure, which greatly improves its chemical stability. The structural synthesis of the asymmetric monomer increases the polarity of the molecular chain, making it easy to adsorb solvents, thereby increasing the solubility of the photosensitive resin precursor resin. At the same time, the substitution of the photosensitive group on the side chain improves the photosensitivity of the cross-linking. Under the preferred ratio, the structure of the polymer main chain is improved, and the problem of high water absorption caused by the structure of polyimide is coordinated to reduce, thereby improving the storage stability of the photosensitive resin system; while participating in the film-forming structure, the rigid benzene ring and heterocyclic ring in the molecule are almost coaxial with the main chain axis, playing a certain strain protection role, and assisting in improving the chemical stability of the photosensitive resin precursor.
[0044] Preferably, the crosslinking agent is at least one of glycidyl acrylate and glycidyl acrylate.
[0045] Preferably, the photoinitiator is at least one of a benzophenone derivative and an acetophenone derivative.
[0046] Preferably, the polymerization inhibitor is at least one of N-phenylnaphthylamine and 4-methoxyphenol.
[0047] Preferably, the silane coupling agent is KH570.
[0048] Preferably, the organic solvent 1 is at least one of N,N-dimethylacetamide and ethyl acetate.
[0049] Preferably, the inorganic filler is a silane-modified inorganic filler.
[0050] Preferably, the preparation steps of the silane-modified inorganic filler are as follows:
[0051] The silane modifier and the inorganic filler are mixed at 200-250° C., air flow is introduced, and dehydration is performed at 100-130° C. to obtain the silane-modified inorganic filler.
[0052] Preferably, the mass ratio of the silane modifier to the inorganic filler is (1-3):50, and the silane modifier is a fluorine-containing silane modifier.
[0053] More preferably, the silane modifier is trifluoromethyltrimethylsilane.
[0054] Preferably, in the step of preparing the silane-modified inorganic filler, the inorganic filler is at least one of mica powder and silicon dioxide, and the mesh size is 100 to 500 meshes.
[0055] More preferably, in the step of preparing the silane-modified inorganic filler, the inorganic filler is mica powder with a mesh size of 300 to 500 meshes.
[0056] The applicant has found that in a system where a silane coupling agent is already present, the addition of a silane-modified inorganic filler can enhance the overall cross-linking network bonding degree, thereby improving the adhesion of the photosensitive resin after curing into a film. Due to the superior compatibility of the fluorinated silane-modified inorganic filler in the system, its smaller molecular structure utilizes the resin voids to increase the cross-linking density, thereby jointly increasing the tensile strength of the system.
[0057] Another aspect of the present invention provides a method for preparing a photosensitive resin having excellent adhesion properties, characterized in that it comprises the following steps:
[0058] Add the photosensitive resin precursor to solvent 1, rinse the precipitated solid with solvent 2, dry it and transfer it to a reactor, then add the crosslinking agent, photoinitiator, inhibitor, silane coupling agent and organic solvent 1 in sequence and mix and stir, then add the inorganic filler and stir thoroughly until it is evenly dispersed to obtain a photosensitive resin.
[0059] Preferably, the solvent 1 is a poor solvent.
[0060] More preferably, the poor solvent is deionized water or methanol.
[0061] Preferably, the solvent 2 is deionized water or methanol.
[0062] Compared with the prior art, the present invention has the following beneficial effects:
[0063] (1) The photosensitive resin with excellent adhesion provided by the present invention regulates the weight average molecular weight of the acrylate polymer through the preferred steps so that when it is used as a part of the main chain of the photosensitive resin precursor, it maintains a certain chain length and density distribution, reduces the adsorption of water, and assists in reducing the water absorption of the photosensitive resin.
[0064] (2) The aromatic ring structure of the main chain of the photosensitive resin precursor with excellent adhesion provided by the present invention improves the chemical stability, and the asymmetry of the monomer polymerization structure increases the polarity of the molecular chain, making it easy to adsorb solvents, thereby increasing the solubility of the photosensitive resin precursor resin.
[0065] (3) The photosensitive resin with excellent adhesion performance provided by the present invention improves the photosensitivity of crosslinking by replacing the photosensitive group on the side chain. At a preferred ratio, the structure of the polymer main chain is improved, the problem of high water absorption caused by polyimide is coordinated to be reduced, and the storage stability of the photosensitive resin system is improved.
[0066] (4) The photosensitive resin with excellent adhesion performance provided by the present invention improves the adhesion of the photosensitive resin after curing into a film by utilizing the effect of improving the overall cross-linking network bonding degree of the silane-modified inorganic filler in the system where a silane coupling agent is already present. In addition, due to the better compatibility of the fluorinated silane-modified inorganic filler in the system and its smaller molecular structure, the cross-linking density is increased by utilizing the resin voids, thereby jointly increasing the tensile strength of the system. DETAILED DESCRIPTION
[0067] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0068] Unless otherwise specified, the reagents used below can be easily obtained from commercial companies.
[0069] Preparation Example 1
[0070] The preparation steps of the photosensitive resin precursor 1 are as follows:
[0071] (1) In a reactor, 0.3 g of acrylic acid, 15 g of methyl methacrylate and 13 g of hydroxyethyl methacrylate were copolymerized in 55 mL of propylene glycol methyl ether acetate, 0.28 g of azobisisobutyronitrile and 4.2 g of basic magnesium carbonate were added, and the mixture was reacted at 60° C. for 5 h to obtain an acrylic ester polymer;
[0072] (2) First, 95 mL of propylene glycol methyl ether acetate, 0.03 g of p-methoxyphenol and 0.4 g of tetraethylammonium bromide were added to the reactor, and then 50 g of acrylate polymer and 0.55 g of methoxyacetophenone were added to the reactor and mixed, and reacted at 15° C. for 8 h to obtain intermediate 1;
[0073] (3) 60 mL of propylene glycol methyl ether acetate and 0.4 mL of sulfuric acid were added to a reactor, 25.3 g of intermediate 1 and 1.6 g of hexafluorodianhydride were mixed and stirred, and the mixture was reacted at room temperature for 7 h to obtain intermediate 2;
[0074] (4) 250 mL of dichloromethane, 52.5 g of intermediate 2, 0.01 mL of N,N-dimethylformamide and 3.0 g of benzoyl chloride were added to the reactor in sequence, reacted at 6°C for 3 h, and reacted at 24°C for 5 h to obtain intermediate 3;
[0075] (5) 1.9 g of diaminodiphenylmethane and 125 mL of propylene glycol methyl ether acetate were added to the reactor and stirred evenly. Then, 54 g of intermediate 3 and 0.3 g of tetrahydrophthalic anhydride were added and mixed. The mixture was stirred and reacted at room temperature for 13 h. Then, 0.04 g of acetic anhydride and 0.03 g of pyridine were added and reacted at 13° C. for 4 h to obtain a photosensitive resin precursor 1.
[0076] Preparation Example 2
[0077] The preparation steps of the photosensitive resin precursor 2 are the same as those of Preparation Example 1, except that in step (3), 1.6 g of hexafluorodianhydride is replaced with 1.7 g of pyromellitic dianhydride to obtain the photosensitive resin precursor 2.
[0078] Preparation Example 3
[0079] The preparation steps of photosensitive resin precursor 2 are the same as those of Preparation Example 1, except that in step (1), methyl methacrylate is 18 g, and photosensitive resin precursor 3 is obtained.
[0080] Preparation Example 4
[0081] The preparation steps of photosensitive resin precursor 2 are the same as those of Preparation Example 1, except that in step (1), methyl methacrylate is 12 g, and photosensitive resin precursor 4 is obtained.
[0082] Preparation Example 5
[0083] 2 g of trifluoromethyltrimethylsilane and 50 g of mica powder were mixed at 220° C., air flow was introduced, and dehydration was performed at 120° C. to obtain silane-modified inorganic filler a.
[0084] Preparation Example 6
[0085] 2 g of trifluoromethyltrimethylsilane and 50 g of silicon dioxide were mixed at 220° C., air flow was introduced, and dehydration was performed at 120° C. to obtain a silane-modified inorganic filler b.
[0086] Example 1
[0087] A photosensitive resin with excellent adhesion performance, the photosensitive resin comprising the following raw materials in parts by weight: 40 parts of a photosensitive resin precursor 1, 25 parts of glycidyl acrylate, 25 parts of benzophenone, 2.5 parts of 4-methoxyphenol, 2.5 parts of KH570, 50 parts of N,N-dimethylacetamide, 60 parts of a silane-modified inorganic filler a, 80 parts of methanol and 100 parts of deionized water.
[0088] The method for preparing the photosensitive resin of this embodiment comprises the following steps:
[0089] The photosensitive resin precursor 1 is added to methanol, the precipitated solid is rinsed with deionized water, dried and transferred to a reactor, and then glycidyl acrylate, benzophenone, 4-methoxyphenol, KH570 and N, N-dimethylacetamide are added in sequence and mixed and stirred, and then the silane-modified inorganic filler a is added and stirred until it is evenly dispersed to obtain a photosensitive resin.
[0090] Example 2
[0091] A photosensitive resin with excellent adhesion performance, the photosensitive resin comprising the following raw materials in parts by weight: 10 parts of a photosensitive resin precursor 1, 2 parts of glycidyl acrylate, 0.01 parts of benzophenone, 0.01 parts of 4-methoxyphenol, 0.01 parts of KH570, 20 parts of N,N-dimethylacetamide, 50 parts of a silane-modified inorganic filler a, 80 parts of methanol and 100 parts of deionized water.
[0092] The preparation method of the photosensitive resin in this embodiment is the same as that in embodiment 1.
[0093] Example 3
[0094] A photosensitive resin with excellent adhesion performance, the photosensitive resin comprising the following raw materials in parts by weight: 70 parts of a photosensitive resin precursor 1, 50 parts of glycidyl acrylate, 50 parts of benzophenone, 5 parts of 4-methoxyphenol, 5 parts of KH570, 80 parts of N,N-dimethylacetamide, 70 parts of a silane-modified inorganic filler a, 80 parts of methanol and 100 parts of deionized water.
[0095] The preparation method of the photosensitive resin in this embodiment is the same as that in embodiment 1.
[0096] Example 4
[0097] A photosensitive resin with excellent adhesion performance and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the photosensitive resin precursor 2 is used to replace the photosensitive resin precursor 1 in equal amounts.
[0098] Example 5
[0099] A photosensitive resin with excellent adhesion performance and a preparation method thereof, the specific implementation manner is the same as that of Example 1, except that the photosensitive resin precursor 1 is replaced by an equal amount of a photosensitive resin precursor 3.
[0100] Example 6
[0101] A photosensitive resin with excellent adhesion performance and a preparation method thereof, the specific implementation manner is the same as that of Example 1, except that the photosensitive resin precursor 4 is used to replace the photosensitive resin precursor 1 in equal amounts.
[0102] Example 7
[0103] A photosensitive resin with excellent adhesion performance and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the silane-modified inorganic filler a is replaced by an equal amount of the silane-modified inorganic filler b.
[0104] Comparative Example 1
[0105] A photosensitive resin with excellent adhesion performance and a preparation method thereof, the specific implementation method is the same as that of Example 1
[0106] The preparation method of the photosensitive resin in this comparative example is the same as that in Example 1, except that the silane-modified inorganic filler a is replaced by an equal amount of inorganic filler, and the inorganic filler is 600-mesh mica powder purchased from Guangdong Yuanlei Powder Co., Ltd.
[0107] Performance Testing:
[0108] The photosensitive resin prepared in the above examples and comparative examples was coated on the surface of the substrate and subjected to exposure, development and thermal curing to form a cured film. The thickness of the cured film was controlled to be about 30 μm, and the following performance tests were performed. The specific test results are shown in Table 1.
[0109] (1) Stability: The cured film was completely immersed in deionized water at room temperature for 24 h and the water absorption rate was tested, which represents the stability of the photosensitive resin.
[0110] (2) Adhesion performance: After making 100 2 mm square holes, the tape peeling test was performed using the cross-cut tape method at 60 mJ / cm 2 The pattern generated by exposure was evaluated, and the number of peeling patterns was measured by optical microscopy, where: O: no peeling on the pattern; A: 1 to 10 peelings on the pattern; X: more than 10 peelings on the pattern.
[0111] (3) Tensile strength: The tensile strength of the cured film was tested using a universal testing machine.
[0112] Table 1
[0113] serial number Water absorption / % Adhesion performance / - Tensile strength / MPa Example 1 0.30 O 99.41 Example 2 0.35 O 97.09 Example 3 0.36 O 98.55 Example 4 0.46 A 95.12 Example 5 0.50 A 94.48 Example 6 0.80 O 96.10 Example 7 0.77 A 90.78 Comparative Example 1 0.89 X 90.54
[0114] As shown in Table 1, the photosensitive resin provided in Examples 1 to 3 of the present invention is a photosensitive resin with good adhesion and tensile properties, low water absorption during development, good storage stability, and has significant beneficial effects.
[0115] Among them, by comparing Example 1 and Example 4, it can be seen that the photosensitive resin provided by the present invention uses fluorine-containing dianhydride to synthesize polyimide, and the presence of fluorine element can significantly reduce the water absorption rate of the photosensitive resin and improve the stability of the photosensitive resin; by comparing Example 1 with Examples 5 and 6, it can be seen that when the monomer polymerization addition amount of methyl methacrylate polymer is inappropriate, the chain length and density distribution of the photosensitive resin are affected. Although the adhesion is improved to a certain extent, its adsorption of water affects the water absorption rate of the photosensitive resin, resulting in a decrease in storage stability; by comparing Example 7 with Example 1, it can be seen that when the addition amount of the fluorine-containing silane modifier is inappropriate, the degree of crosslinking after curing of the silane coupling agent in the system is adversely affected, thereby affecting the tensile strength of the cured film of the photosensitive resin; by comparing Example 1 with Comparative Example 1, it can be seen that the silane-modified mica powder with a preferred mesh size provided by the present invention has a low moisture content and has better compatibility in the photosensitive resin system. Its smaller molecular structure increases the crosslinking density by utilizing the resin voids, and together increases the tensile strength of the system.
[0116] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.
Claims
1. A photosensitive resin with excellent adhesion properties, It is characterized in that The photosensitive resin comprises the following raw materials in parts by weight: 10 to 70 parts of a photosensitive resin precursor, 2 to 50 parts of a crosslinking agent, 0.01 to 50 parts of a photoinitiator, 0.01 to 5 parts of a polymerization inhibitor, 0.01 to 5 parts of a silane coupling agent, 20 to 80 parts of an organic solvent 1, 50 to 70 parts of an inorganic filler, 20 to 100 parts of a solvent 1 and 50 to 200 parts of a solvent 2. Wherein, the inorganic filler is a silane-modified inorganic filler.
2. The photosensitive resin having excellent adhesion properties according to claim 1, It is characterized in that The preparation steps of the photosensitive resin precursor are as follows: (1) in a reactor, acrylic acid, acrylic acid ester monomer, and acrylic acid hydroxyl monomer are copolymerized in an organic solvent 2, an initiator and a dispersant are added, and the mixture is reacted at 50 to 70° C. for 4 to 6 hours to obtain an acrylic acid ester polymer; (2) firstly adding a first weight portion of an organic solvent 2, a polymerization inhibitor and a catalyst 1 into a reactor, then adding the acrylic ester polymer and the benzene ring-containing ketone compound into the reactor and mixing them, reacting at 0 to 30° C. for 6 to 10 hours to obtain an intermediate 1; (3) Adding a second weight portion of organic solvent 2 and catalyst 2 into the reactor, mixing the intermediate 1 with the dianhydride and stirring, and reacting at room temperature for 4 to 10 hours to obtain intermediate 2. (4) adding organic solvent 3, intermediate 2, catalyst 3 and acyl chloride reagent to the reactor in sequence, reacting at 0-12° C. for 1-5 h, and reacting at 22-26° C. for 2-8 h to obtain intermediate 3; (5) Add diamine and the third part by weight of organic solvent 2 into the reactor and stir evenly, then add intermediate 3 and molecular weight regulator and mix, stir and react at room temperature for 10 to 16 hours, then add dehydrating agent and catalyst 4, react at 0 to 25° C. for 2 to 6 hours to obtain a photosensitive resin precursor.
3. The photosensitive resin having excellent adhesion properties according to claim 2, It is characterized in that The amount of acrylic acid monomer added in step (1) is 1 to 1.2% of the total mass of acrylic acid ester monomer and acrylic acid hydroxyl monomer.
4. The photosensitive resin having excellent adhesion properties according to claim 2, It is characterized in that The amount of the dispersant added in step (1) is 10-40% of the total mass of the acrylic acid monomer, the acrylic ester monomer and the acrylic hydroxyl monomer.
5. The photosensitive resin having excellent adhesion properties according to claim 2, It is characterized in that The ketone compound containing a benzene ring in the step (2) is an ethyl ketone compound containing a benzene ring.
6. The photosensitive resin having excellent adhesion properties according to claim 2, It is characterized in that In the step (3), the molar ratio of the intermediate 1 to the dianhydride is 1:(1.2-1.8), and in the step (4), the molar ratio of the intermediate 2 to the acyl chloride reagent is 1:(2-2.2).
7. The photosensitive resin having excellent adhesion properties according to claim 2, It is characterized in that In the step (5), the molar ratio of the intermediate 3, the diamine and the molecular weight regulator is 1: (0.8-1.1): (0.01-0.5).
8. The photosensitive resin having excellent adhesion properties according to claim 1, It is characterized in that The preparation steps of the silane-modified inorganic filler are as follows: The silane modifier and the inorganic filler are mixed at 200-250° C., air flow is introduced, and dehydration is performed at 100-130° C. to obtain the silane-modified inorganic filler.
9. The photosensitive resin having excellent adhesion properties according to claim 8, It is characterized in that The mass ratio of the silane modifier to the inorganic filler is (1-3):50, and the silane modifier is a fluorine-containing silane modifier.
10. A method for preparing the photosensitive resin having excellent adhesion properties according to any one of claims 1 to 9, It is characterized in that The following steps are involved: Add the photosensitive resin precursor to solvent 1, rinse the precipitated solid with solvent 2, dry it and transfer it to a reactor, then add the crosslinking agent, photoinitiator, inhibitor, silane coupling agent and organic solvent 1 in sequence and mix and stir, then add the inorganic filler and stir thoroughly until it is evenly dispersed to obtain a photosensitive resin.