Phytic acid mediated degradable protein gel electrolyte as well as preparation method and application thereof

By introducing sodium chloride and EDC into gelatin protein gel and using phytic acid mediation at high salt concentrations to form a strong interaction force, the mechanical properties and biocompatibility of gel electrolytes are solved, and high performance is achieved Supercapacitor material, and the material is degradable and environmentally friendly.

CN118919310APending Publication Date: 2024-11-08SHANDONG AGRICULTURAL UNIVERSITY

Patent Information

Application Number
CN202411077324.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing gel electrolytes have poor mechanical properties, high cost, poor biocompatibility, difficult to degrade and cause environmental pollution.

Method used

Amidation by introducing sodium chloride and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide (EDC) into gelatin proteins using phytic acid-mediated degradable protein gel electrolytes Cross-linking and phytic acid is introduced at high salt concentrations to form a strong interaction force, improving the mechanical properties and biocompatibility of the gel.

Benefits of technology

It significantly improves the mechanical and electrochemical properties of the gel, is suitable for supercapacitors, has good rate characteristics and cycle life, and is simple in preparation, low in cost, degradable material, and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919310A_ABST
    Figure CN118919310A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of new energy electrolyte materials, and particularly relates to a phytic acid mediated degradable protein gel electrolyte and a preparation method and application thereof.The electrolyte is mainly prepared from gelatin protein, sodium chloride, phytic acid, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide and water; due to the fact that a chemical cross-linked network formed by introducing the cross-linking agent and a physical cross-linked network formed by protein precipitation triggered after introduction of phytic acid construct a chemical and physical cross-linked double-network structure together, the toughening effect on the gel is remarkable, the mechanical performance of the gel can be further enhanced, and the gel has excellent mechanical performance and electrochemical performance; the material has a series of advantages of good rate capability, long cycle life and the like when being used as a supercapacitor electrolyte material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of new energy electrolyte materials and relates to a protein gel electrolyte, and more specifically to a phytic acid-mediated degradable protein gel electrolyte and a preparation method and application thereof. Background Art

[0002] In recent years, with the widespread application of portable wearable and implantable smart devices in sports, medical health and other fields, the development of flexible supercapacitors and other energy storage devices that are compatible with them has become an important research goal. Unlike traditional energy storage devices, wearable and implantable supercapacitors must have biosafety and compatibility. In addition, according to different working requirements and types, their functions must be adjusted according to actual conditions, such as their size, shape, mechanical properties, natural degradation conditions, and operating temperature range, in order to cope with the challenges of different situations.

[0003] Gel electrolytes have mechanical flexibility similar to that of solids and high ion mobility similar to that of liquids, making them ideal materials for building flexible energy storage devices. Traditional gel electrolytes are assembled from high molecular polymers, such as polyvinylidene fluoride (PVDF), polyethylene oxide (PEO), and polyvinyl alcohol (PVA). However, on the one hand, some high molecular polymers are extracted from fossil fuels, which will cause a large amount of carbon emissions during the manufacturing process; on the other hand, some high molecular polymers are difficult to degrade in the body and have high biological toxicity. In addition, since some devices use toxic and corrosive electrolytes, energy storage devices must be strictly encapsulated, which increases the size of medical electronic equipment and brings difficulties and pain to patients during implantation.

[0004] As a natural high molecular polymer, protein is renewable, widely available, easy to process and has good biocompatibility. Almost all of them can be decomposed by microorganisms under natural conditions, and the decomposition products can be used as nutrients for animals and plants to absorb. The surface of protein chains is rich in polar functional groups such as carboxyl, amino and hydroxyl groups, which can interact with carriers to improve salt solubility and ion transport properties. However, the mechanical properties of conventional protein gel electrolytes are poor, which seriously limits the electrochemical performance and application flexibility of electrochemical energy storage devices. The properties of gel electrolytes can be further improved by physical cross-linking or chemical cross-linking methods, such as surface functional group grafting to modify protein precursors, or by constructing interpenetrating polymer networks with other traditional polymers. However, the introduced modifiers or complexes usually have an adverse effect on the biocompatibility of the gel, and the conventional modification methods are complicated and difficult to meet actual production needs.

[0005] CN117487199A discloses a method for preparing a gelatin-based gel electrolyte with a double network structure. First, a gelatin solution is prepared, and then a certain amount of high molecular polymer is weighed and mixed with the gelatin solution, and then an alkaline solution is added. After standing, a double network stable electrolyte is obtained. However, the electrolyte still has the problems of poor mechanical properties and high cost. In addition, since the preparation process still needs to introduce other high molecular polymer components into the polymer network, it needs to be treated with an alkaline solution later. The biocompatibility of the gel is poor, it is difficult to degrade, and it has certain pollution.

[0006] Therefore, research on protein gel electrolytes with better performance has become the focus of research for those skilled in the art. Summary of the invention

[0007] In order to overcome the problems of poor mechanical properties, high cost, poor biocompatibility, difficulty in degradation and environmental pollution of gel electrolytes in the prior art, the present invention provides a phytic acid-mediated degradable protein gel electrolyte and a preparation method thereof. The gel electrolyte is used in supercapacitors, showing high specific capacity and high rate characteristics, which can promote the application of high-performance supercapacitors.

[0008] There are two general modification schemes for protein gels with poor mechanical properties. One is to design a special structure, and the other is to introduce some other polymers to improve the mechanical properties of the gel. Compared with this, the modification strategy adopted by the present invention is simpler. It only needs to use phytic acid to induce salting out of the protein, and the introduced phytic acid can also form a strong interaction force with the protein peptide chain. There is no need to design a complicated modification strategy or introduce other polymers, thereby continuing the good biocompatibility of the protein material.

[0009] Therefore, the present invention first provides a phytic acid mediated degradable protein gel electrolyte, whose main components are gelatin protein, sodium chloride, phytic acid, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide (EDC) and water, wherein the content of gelatin protein relative to water is between 100 and 500 mg / ml, and the mass ratio of gelatin protein to EDC should be 10:1; the content of sodium chloride relative to water is 1 to 5M, and the content of phytic acid is 3-5 mg / ml.

[0010] Moreover, as the sodium chloride concentration increases, the gel salting-out effect becomes more significant, which increases the relative protein content and leads to improved mechanical properties of the prepared samples. When the sodium chloride concentration in the gel is 5M, the prepared gel sample can exhibit a stress of more than 1.8MPa when compressed to 90%.

[0011] The phytic acid used is a very important natural substance, which is widely found in plants such as beans, cereals, dried fruits, vegetables and fruits. It has a wide source and will not cause secondary pollution to the environment during the degradation process.

[0012] In addition, the inventors also provide a method for preparing the above-mentioned phytic acid-mediated degradable protein gel electrolyte, the steps of which are as follows:

[0013] 1) Dissolve gelatin and sodium chloride in deionized water at a certain mass ratio, and stir at a constant temperature to obtain a transparent mixed solution;

[0014] 2) adding a certain concentration of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide (EDC) aqueous solution to the mixed solution obtained in step 1) in proportion, and coating to obtain a gel electrolyte with a certain thickness;

[0015] 3) Soaking the gel electrolyte obtained in step 2) in a solution containing a certain concentration of sodium chloride and phytic acid to obtain a phytic acid-mediated degradable protein gel electrolyte.

[0016] The preparation method first uses 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide (EDC) to perform amidation crosslinking in a solution containing gelatin protein and sodium chloride, and after the crosslinking agent is introduced, the hydroxyl and amino groups on the gelatin protein peptide chain are crosslinked to form a transparent gel; on this basis, phytic acid is introduced to diffuse into the protein crosslinking network and interact strongly with the protein chain, and the phytic acid enters between the protein peptide chains, so that the chains aggregate, precipitate, and salting out effect occurs; during the whole process, the presence of sodium chloride destroys the original hydration layer between the protein peptide chains, so that the distance between the peptide chains becomes shorter and easy to aggregate, and when the salt concentration is high, the protein self-assembly can be effectively prevented, so that the original solution in step 1) is always kept in a solution state, and after the subsequent amidation crosslinking, the introduction of phytic acid makes it easier for the peptide chains to aggregate and precipitate, thereby significantly improving the mechanical properties of the gel electrolyte.

[0017] Preferably, in the step 1), 0.4-0.6 g of gelatin and 0.23-1.75 g of sodium chloride are weighed and added to 4-6 mL of deionized water; the gelatin is industrial gelatin; and in the step 1), magnetic stirring is performed at 50-65° C. until the gelatin is dissolved into a transparent solution.

[0018] Preferably, in the step 2), after the mixed solution obtained in step 1) is cooled to room temperature, 80 to 120 μL of an EDC solution with a concentration of 500 mg / mL is added thereto while stirring, and the mixture is evenly dispersed; the evenly dispersed dispersion is coated on a polytetrafluoroethylene mold, and allowed to stand at room temperature for 1 to 2 hours to deepen the degree of crosslinking, and then removed from the polytetrafluoroethylene mold to obtain a complete gel sheet with a thickness of 0.8 to 1 cm;

[0019] In addition to the above-mentioned gel sheets, it can also be prepared into cylindrical gel blocks as needed by simply replacing the corresponding mold, such as pouring the evenly dispersed dispersion into a mold lined with polytetrafluoroethylene, and taking out the cylindrical gel block from the mold.

[0020] Preferably, in the step 3), 4.09-27.47 g of sodium chloride and 0.73-7.14 g of a phytic acid solution with a mass fraction of 70% are weighed, added to 100-200 mL of deionized water and mixed evenly to prepare a soaking solution for gel modification; then the gel electrolyte prepared in step 2) is soaked in the above-mentioned soaking solution for gel modification for 6-12 hours to obtain a phytic acid-mediated degradable protein gel electrolyte.

[0021] In step 1), if the sodium chloride concentration is too low or the gelatin concentration is too high, the shielding effect of sodium chloride on the interaction between gelatin protein peptide chains may be weakened, causing gelatin to self-assemble into a gel at room temperature, affecting the subsequent introduction of a cross-linking agent and increasing the difficulty of the process preparation.

[0022] In the step 3), as the amount of sodium chloride changes, the content of sodium chloride in the soaked gel sample will also change due to osmotic pressure and other reasons; in the step 3), as the concentration of phytic acid increases, the acidity in the soaking solution gradually increases, which will destroy the amide bonds in the protein, making it impossible for the gelatin protein gel to maintain its complete shape.

[0023] The phytic acid-mediated degradable protein gel electrolyte prepared by the above method can be applied to the field of gel electrolytes for supercapacitors. More specifically, the protein gel electrolyte is directly used to replace conventional liquid or solid electrolytes.

[0024] The electrolyte materials used in existing conventional capacitors are liquid or solid materials, and the liquid phase needs to add a diaphragm to prevent short circuit. The present invention uses protein gel electrolyte to replace conventional liquid or solid electrolytes, while inheriting the high ionic conductivity of the liquid phase and the advantages of the solid phase. At the same time, protein is rarely used as a base material in the prior art, and the few gel electrolytes prepared using protein materials also need to add other polymers to enhance the mechanical properties. The technical solution of the present application does not introduce other polymer modifications, inherits the environmental friendliness of protein, and meets the needs of gel electrolytes for supercapacitors.

[0025] Compared with the prior art, the preparation of phytic acid-mediated degradable protein gel electrolyte by the scheme of the present invention achieves the following technical effects:

[0026] 1) Before constructing the gel cross-linking network, high concentration of sodium chloride is used to shield the interaction between gelatin protein chains, which can prevent the cross-linking of gelatin at room temperature from affecting subsequent operations;

[0027] 2) EDC was introduced to amidate the gelatin peptide chains. The constructed cross-linked network could not only maintain high ionic conductivity, but also effectively improve the mechanical stability and thermal stability of the gel sheet. EDC was used to perform amidation cross-linking in a solution containing gelatin protein and NaCl. On this basis, phytic acid was introduced to diffuse into the protein cross-linked network and interact strongly with the protein chains.

[0028] 3) The phosphorus hydroxyl group introduced into phytic acid will form a strong interaction force with the hydroxyl group and amino group on the peptide chain. Due to the presence of NaCl, the hydration layer thickness of the protein chain is reduced. The protein chains are close to each other and further aggregated under the action of hydrogen bonds. Then, due to the presence of hydrophobic interactions, ionic bonds and other forces, the protein chains are precipitated, thereby significantly improving the mechanical properties of the gel electrolyte. The chemical cross-linking network formed by the introduction of the cross-linking agent and the physical cross-linking network formed by the protein precipitation triggered by the introduction of phytic acid together construct a chemical and physical cross-linking double network structure, which has a significant toughening effect on the gel and can further enhance the mechanical properties of the gel. Therefore, the material has both excellent mechanical properties and electrochemical properties. It has a series of advantages such as good rate characteristics and long cycle life when used as a supercapacitor electrode material.

[0029] 4) The preparation method has a simple and safe operation process, a simple process, low equipment cost, and easy-to-obtain raw materials. The cost is low and easy to industrialize. The gelatin and phytic acid raw materials are widely available, degradable, and have good biocompatibility. It will not cause secondary pollution to the environment and can provide a high-performance implantable supercapacitor gel electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 These are the compression performance test results of the phytic acid-mediated degradable protein gel electrolytes prepared in Examples 1, 2, 4, and 5 of the present invention;

[0031] Figure 2 is the infrared spectrum of the gel material prepared in Examples 1-5 of the present invention;

[0032] Figure 3 is the monitoring result of the gel material preparation process in Example 6 of the present invention;

[0033] Figure 4 is a SEM image of a freeze-dried material prepared from the phytic acid-mediated degradable protein gel electrolyte prepared in Example 7 of the present invention;

[0034] Figure 5 is the test result of the electrochemical performance of the phytic acid-mediated degradable protein gel electrolyte prepared in Example 8 of the present invention after being loaded into a supercapacitor, wherein Figure 5 a is the impedance curve spectrum, Figure 5 b is the volt-ampere characteristic cycle curve, Figure 5c is the charge and discharge curve at different current densities. Figure 5 d is the capacitance cycle stability diagram;

[0035] Figure 6 The phytic acid-mediated degradable protein gel electrolyte prepared in Example 9 of the present invention is loaded into a supercapacitor at 1Ag -1 The test results after 60,000 cycles at a rate of;

[0036] Figure 7 The degradation of the phytic acid-mediated degradable protein gel electrolyte prepared in Example 11 of the present invention under simulated gastric fluid;

[0037] Figure 8 This is the degradation of the phytic acid-mediated degradable protein gel electrolyte prepared in Example 12 of the present invention under simulated natural conditions. DETAILED DESCRIPTION

[0038] The technical solution of the present invention is further described below in conjunction with specific embodiments. These embodiments are only used to illustrate the technical solution of the present invention in more detail and should not be construed as limiting the protection scope of the present invention.

[0039] The gelatin, EDC, and phytic acid solution used in the examples are all from Shanghai Aladdin Biochemical Technology Co., Ltd., wherein the main raw material of gelatin is bovine bone; the other substances and reagents used are all generally commercially available products.

[0040] Example 1

[0041] A method for preparing a degradable protein gel electrolyte, the specific steps are as follows:

[0042] Weigh 0.4 g of gelatin particles and 1.17 g of sodium chloride, add them to 4 mL of deionized water, and stir them with a constant temperature magnetic stir at 55°C until they are completely dissolved. After cooling to room temperature, add 80 uL of 500 mg / mL EDC solution while stirring, pour into a mold lined with polytetrafluoroethylene, let stand at room temperature for 1 h, and take it out from the mold to obtain a cylindrical gel block; this sample is named G.

[0043] The thickness and area of ​​the gel were measured, and the compression performance of the prepared gel samples was tested at a speed of 1 mm / min. Some samples were taken for infrared spectrum testing. The results were as follows: Figure 1 , 2 shown.

[0044] Example 2

[0045] A method for preparing a degradable protein gel electrolyte, the specific steps are as follows:

[0046] Weigh 0.5 g of gelatin particles and 0.29 g of sodium chloride, add them to 5 mL of deionized water, and stir them with a constant temperature magnetic stir at 65°C until they are completely dissolved. After cooling to room temperature, add 100 uL of 500 mg / mL EDC solution while stirring, pour into a mold lined with polytetrafluoroethylene to fix the thickness and let stand at room temperature for 1.5 h. Take it out from the mold to obtain a cylindrical gel block; this sample is named GE-1.

[0047] The thickness and area of ​​the gel were measured, and the compression performance of the prepared gel samples was tested at a speed of 1 mm / min. Some samples were taken for infrared spectrum testing. The results were as follows: Figure 1 , 2 shown.

[0048] Judging from the test results of sample compression performance, the chemical cross-linking network initially constructed after the introduction of the cross-linking agent also improves the mechanical properties of the sample to a certain extent.

[0049] Example 3

[0050] A method for preparing a degradable protein gel electrolyte, the specific steps are as follows:

[0051] Weigh 0.4 g of gelatin particles and 1.17 g of sodium chloride, add them to 4 mL of deionized water, and stir them with a constant temperature magnetic force at 55°C until they are completely dissolved. After cooling to room temperature, add 80 uL of 500 mg / mL EDC solution while stirring. Apply the evenly dispersed dispersion on a polytetrafluoroethylene mold, fix the thickness, and let it stand at room temperature for 1.5 hours to obtain a gel sheet with a thickness of 0.8 cm. The sample was named GE-5 and subjected to infrared spectrum testing. The results are as follows: Figure 2 shown.

[0052] Example 4

[0053] A method for preparing a degradable protein gel electrolyte, the specific steps are as follows:

[0054] Weigh 0.4 g of gelatin particles and 1.17 g of sodium chloride, add them to 4 mL of deionized water, stir them with a constant temperature magnetic stirrer at 55 °C until they are completely dissolved, add 80 uL of 500 mg / mL EDC solution while stirring after cooling to room temperature, pour into a mold lined with polytetrafluoroethylene to fix the thickness and let stand at room temperature for 1.5 h, take it out from the mold to obtain a cylindrical gel block;

[0055] Weigh 0.74 g of 70% phytic acid solution and 5.8 g of sodium chloride, add them into 100 mL of deionized water, mix them evenly to make a soaking solution, soak the obtained cylindrical gel block in the soaking solution for 6 hours to obtain a phytic acid-mediated degradable protein gel electrolyte; the sample is named GEP-1.

[0056] The thickness and area of ​​the gel were measured, and the compression performance of the prepared gel samples was tested at a speed of 1 mm / min. Some samples were taken for infrared spectrum testing. The results were as follows: Figure 1 , 2 shown.

[0057] Judging from the test results of sample compression performance, compared with samples G and GE-1, the mechanical properties of sample GEP-1 have been greatly improved. It can still maintain its complete shape after deformation of 90%, and the stress has also been greatly improved under the same strain.

[0058] Example 5

[0059] A method for preparing a phytic acid-mediated degradable protein gel electrolyte, the specific steps are as follows:

[0060] Weigh 0.4 g of gelatin particles and 1.17 g of sodium chloride, add them to 4 mL of deionized water, stir them with a constant temperature magnetic stirrer at 55 °C until they are completely dissolved, add 80 uL of 500 mg / mL EDC solution while stirring after cooling to room temperature, pour into a mold lined with polytetrafluoroethylene to fix the thickness and let stand at room temperature for 1.5 h, take it out from the mold to obtain a cylindrical gel block;

[0061] Weigh 0.74 g of 70% phytic acid solution and 27.47 g of sodium chloride, add them into 100 mL of deionized water, mix them evenly to make a soaking solution, soak the obtained cylindrical gel block in the soaking solution for 6 hours to obtain a phytic acid-mediated degradable protein gel electrolyte; the sample is named GEP-5.

[0062] The thickness and area of ​​the gel were measured, and the compression performance of the prepared gel samples was tested at a speed of 1 mm / min. Some samples were taken for infrared spectrum testing. The results were as follows: Figure 1 , 2 shown.

[0063] Judging from the test results of sample compression performance, sample GEP-5 showed the best compression performance, that is, with the increase of salt concentration in the immersion solution, the mechanical properties of the sample were greatly improved. This can be attributed to the fact that with the increase of salt concentration, the salting-out effect in the sample is more obvious, which can provide better mechanical properties.

[0064] From the infrared spectrum, we can see that in the range of 1633-1626cm -1The characteristic peak at 1548-1536cm has an obvious red shift as the concentration of sodium chloride introduced into the sample increases, and the peak intensity gradually becomes stronger. This peak is the characteristic peak of CH bending vibration in the first region of gelatinamide, indicating that sodium chloride will destroy the original hydrogen bonding force between protein peptide chains, and as the salting-out effect increases, the water content in the sample decreases, resulting in enhanced protein signals. -1 The characteristic peak at appears with the introduction of phytic acid into the sample, and with the increase of sodium chloride concentration, the peak position has an obvious red shift, and the peak intensity gradually becomes stronger. This peak is the NH bending vibration peak of the second zone of gelatinamide, indicating that after sodium chloride weakens the hydration layer between protein peptide chains, the introduction of phytic acid leads to the enhancement of the interaction between protein peptide chains inside the sample, the proteins are close to each other, and the excess water is analyzed out. The inventors tested the infrared spectrum of the phytic acid solution used and named the test results PA. The results are as follows Figure 2 c; at 945cm -1 The characteristic peak of phytic acid is at 975 cm-1. -1 The intensity increases with the increase of salt concentration, indicating that the interaction between phytic acid and protein becomes stronger with the increase of salt concentration.

[0065] Example 6

[0066] A method for preparing a phytic acid-mediated degradable protein gel electrolyte, the specific steps are as follows:

[0067] Weigh 0.4 g of gelatin particles and 1.17 g of sodium chloride, add them to 4 mL of deionized water, stir them with a constant temperature magnetic force at 55°C until they are completely dissolved, add 80 uL of 500 mg / mL EDC solution while stirring after cooling to room temperature, apply the evenly dispersed dispersion on a polytetrafluoroethylene mold, fix the thickness and let it stand at room temperature for 1.5 h, take it out from the mold, and obtain a gel sheet with a thickness of 0.8 cm;

[0068] Weigh 0.74g of phytic acid solution with a mass fraction of 70% and 15.78g of sodium chloride, add them to 100mL of deionized water to prepare a soaking solution; take a part of the gel slice and observe the crystallization inside the gel under a polarizing microscope; drop the soaking solution on the gel slice and observe the change in the degree of gel crystallization during the process of phytic acid entering the gel sample. The results are as follows Figure 3 shown.

[0069] The results showed that the introduction of phytic acid induced a salting-out effect on the protein in the gel, which was manifested in the gradual deepening of the crystallinity in the gel sample with the immersion time, and the gradual reduction of the gel volume due to the tightening of the protein network.

[0070] Example 7

[0071] A method for preparing a phytic acid-mediated degradable protein gel electrolyte, the specific steps are as follows:

[0072] Weigh 0.4 g of gelatin particles and 0.23 g of sodium chloride, add them to 4 mL of deionized water, stir them with a constant temperature magnetic force at 60°C until they are completely dissolved, add 80 uL of 500 mg / mL EDC solution while stirring after cooling to room temperature, apply the evenly dispersed dispersion on a polytetrafluoroethylene mold, fix the thickness and let it stand at room temperature for 2 hours, take it out from the mold, and obtain a gel sheet with a thickness of 0.8 cm;

[0073] Weigh 1.43 g of phytic acid solution with a mass fraction of 70% and 11.69 g of sodium chloride, add them into 200 mL of deionized water, mix them evenly to prepare a soaking solution, and soak the obtained gel sheet in the soaking solution for 6 hours to obtain a phytic acid-mediated degradable protein gel electrolyte.

[0074] The gel electrolyte was rapidly cooled using liquid nitrogen to ensure the integrity of the internal structure during the freeze-drying process of the sample, and then placed in a freeze dryer for vacuum freeze-drying; the obtained freeze-dried material was tested by scanning electron microscopy, and the results were as follows: Figure 4 As shown, a clear pore structure can be observed.

[0075] Example 8

[0076] A method for preparing a phytic acid-mediated degradable protein gel electrolyte, the specific steps are as follows:

[0077] Weigh 0.5 g of gelatin particles and 1.46 g of sodium chloride, add them to 5 mL of deionized water, stir them with a constant temperature magnetic force at 65 °C until they are completely dissolved, add 100 uL of 500 mg / mL EDC solution while stirring after cooling to room temperature, apply the evenly dispersed dispersion on a polytetrafluoroethylene mold, fix the thickness and let it stand at room temperature for 1 h, take it out from the mold, and obtain a gel sheet with a thickness of 1 cm;

[0078] Weigh 0.74 g of phytic acid solution with a mass fraction of 70% and 4.09 g of sodium chloride, add them into 100 mL of deionized water, mix them evenly to prepare a soaking solution, and soak the obtained gel sheet in the soaking solution for 6 hours to obtain a phytic acid-mediated degradable protein gel electrolyte.

[0079] The above gel electrolyte was cut into a circular gel electrolyte sheet with a diameter of 16 mm as the gel electrolyte of the supercapacitor. Activated carbon, acetylene black and polytetrafluoroethylene were mixed evenly in a mass ratio of 8:1:1, pressed into a uniform thin sheet by a rolling method and cut into a raw sheet with a diameter of 10 mm to obtain an electrode sheet. Using a titanium mesh as a current collector, an electrode sheet with a mass of 1.76 mg was pressed into the titanium mesh as the working electrode of the supercapacitor. The basic electrochemical performance test of the supercapacitor was carried out, and the results are as follows: Figure 5 As shown, Figure 5 a is the impedance curve spectrum, Figure 5 b is the volt-ampere characteristic cycle curve, Figure 5 c is the charge and discharge curve at different current densities. Figure 5 d is the capacitance cycle stability diagram.

[0080] For the impedance test, the supercapacitor showed an extremely low resistance; through the CV curve, it was found that it could still maintain a relatively complete rectangular structure at a scan rate of 500mV / s; through the GCD curve results, the supercapacitor was able to ensure cycle stability at a small current of 0.2A / g and a large current of 10A / g; according to the capacitance cycle stability diagram, at a current density of 1A / g, its capacitance retention rate reached more than 99% after 10,000 cycles.

[0081] Example 9

[0082] A method for preparing a phytic acid-mediated degradable protein gel electrolyte, the specific steps are as follows:

[0083] Weigh 0.5 g of gelatin particles and 1.46 g of sodium chloride, add them to 5 mL of deionized water, stir them with a constant temperature magnetic force at 55°C until they are completely dissolved, add 100 uL of 500 mg / mL EDC solution while stirring after cooling to room temperature, apply the evenly dispersed dispersion on a polytetrafluoroethylene mold, fix the thickness and let it stand at room temperature for 1 hour, take it out from the mold, and obtain a gel sheet with a thickness of 1 cm;

[0084] Weigh 0.74 g of phytic acid solution with a mass fraction of 70% and 16.07 g of sodium chloride, add them into 100 mL of deionized water, mix them evenly to prepare a soaking solution, and soak the obtained gel sheet in the soaking solution for 6 hours to obtain a phytic acid-mediated degradable protein gel electrolyte.

[0085] The above gel electrolyte was cut into a circular gel electrolyte sheet with a diameter of 16 mm as the gel electrolyte of the supercapacitor. Activated carbon, acetylene black and polytetrafluoroethylene were mixed evenly in a mass ratio of 8:1:1, pressed into a uniform thin sheet by a rolling method and cut into a raw sheet with a diameter of 10 mm to obtain an electrode sheet. Using a titanium mesh as a current collector, an electrode sheet with a mass of 1.76 mg was pressed into the titanium mesh as the working electrode of the supercapacitor. The long cycle performance of the supercapacitor was tested. Figure 6 As shown, at a current density of 1 A / g, the capacitance retention rate reaches more than 99% after 60,000 cycles.

[0086] Example 10

[0087] A method for preparing a phytic acid-mediated degradable protein gel electrolyte, the specific steps are as follows:

[0088] Weigh 0.6 g of gelatin particles and 1.75 g of sodium chloride, add them to 4 mL of deionized water, stir them with a constant temperature magnetic force at 55°C until they are completely dissolved, add 120 uL of 500 mg / mL EDC solution while stirring after cooling to room temperature, apply the evenly dispersed dispersion on a polytetrafluoroethylene mold, fix the thickness and let it stand at room temperature for 1 hour, take it out from the mold, and obtain a gel sheet with a thickness of 0.8 cm;

[0089] 7.14 g of phytic acid solution with a mass fraction of 70% and 5.84 g of sodium chloride were weighed, added to 100 mL of deionized water, and mixed evenly to make an immersion solution. The obtained gel slices were soaked in the immersion solution for 6 hours to obtain a modified gel. However, due to the high concentration of phytic acid in the immersion solution, the acidity was too strong to destroy the original amide bonds in the gelatin protein, so that the prepared gel sample could not maintain its intact structure and exhibited a latex-like morphology.

[0090] Embodiment 11

[0091] A method for preparing a phytic acid-mediated degradable protein gel electrolyte, the specific steps are as follows:

[0092] Weigh 0.6 g of gelatin particles and 1.75 g of sodium chloride, add them to 6 mL of deionized water, stir them at a constant temperature of 60 ° C with magnetic stirring until they are completely dissolved, add 100 μL of low-concentration crystal violet solution while stirring after cooling to room temperature, and then add 120 uL of 500 mg / mL EDC solution dropwise, apply the evenly dispersed dispersion on a polytetrafluoroethylene mold, fix the thickness and let it stand at room temperature for 1 hour, take it out from the mold, and obtain a purple gel sheet with a thickness of 1 cm;

[0093] Weigh 1.43 g of phytic acid solution with a mass fraction of 70% and 11.69 g of sodium chloride, add them into 200 mL of deionized water, mix them evenly to prepare a soaking solution, and soak the obtained gel sheet in the soaking solution for 6 hours to obtain a phytic acid-mediated degradable protein gel electrolyte.

[0094] Weigh 4 g of porcine pepsin, add it to 400 mL of hydrochloric acid aqueous solution with a pH of 1.5, and drop a trace amount of methyl orange solution therein to prepare simulated gastric fluid; immerse the gel electrolyte in the simulated gastric fluid, stir at a constant temperature of 87 r / min at 37°C, and the gel electrolyte is completely degraded in the simulated gastric fluid after 3 hours. The results are as follows: Figure 7 shown.

[0095] Example 12

[0096] A method for preparing a phytic acid-mediated degradable protein gel electrolyte, the specific steps are as follows:

[0097] Weigh 0.4 g of gelatin particles and 1.17 g of sodium chloride, add them to 4 mL of deionized water, stir them with a constant temperature magnetic stirrer at 65°C until they are completely dissolved, add 100 μL of low-concentration crystal violet solution to it while stirring after cooling to room temperature, and then add 80 μL of 500 mg / mL EDC solution dropwise, apply the evenly dispersed dispersion on a polytetrafluoroethylene mold, fix the thickness and let it stand at room temperature for 1.5 hours, take it out from the mold, and obtain a purple gel sheet with a thickness of 1 cm;

[0098] Weigh 0.74 g of phytic acid solution with a mass fraction of 70% and 5.84 g of sodium chloride, add them into 100 mL of deionized water, mix them evenly to prepare a soaking solution, and soak the obtained gel sheet in the soaking solution for 6 hours to obtain a phytic acid-mediated degradable protein gel electrolyte.

[0099] The gel electrolyte was shallowly buried in a flowerpot, wherein the soil in the flowerpot was prepared by mixing the vegetable-growing nutrient soil from Kunning Wang Gardening with natural soil in a volume ratio of 1:1; wherein the green plants in the flowerpot were from the longevity bamboo sold locally, simulating the degradation process of the gel electrolyte under natural conditions, and the results were as follows Figure 8 As shown, the prepared gel electrolyte was almost completely degraded (changed from purple to colorless) after 18 days.

[0100] In summary, the phytic acid-mediated degradable protein gel electrolyte provided by the present invention can maintain high ionic conductivity and can effectively improve the mechanical stability and thermal stability of the gel sheet. It can be used as a supercapacitor electrode material with a series of advantages such as good rate characteristics and long cycle life. The preparation method has a simple and safe operation process, a simple process, low equipment cost, and easy-to-obtain raw materials. The cost is low and it is easy to industrialize. The gelatin and phytic acid raw materials are widely available, degradable and have good biocompatibility, and will not cause secondary pollution to the environment.

[0101] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any equivalent substitutions, modifications, etc. made by technicians in this field without any creative work within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A phytic acid-mediated degradable protein gel electrolyte, characterized in that: Its main components are gelatin protein, sodium chloride, phytic acid, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide and water, wherein the content of gelatin protein relative to water is between 100 and 500 mg / ml, and the mass ratio of gelatin protein to 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide should be 10:1; the content of sodium chloride relative to water is 1 to 5M, and the content of phytic acid is 3-5 mg / ml.

2. The method for preparing the phytic acid-mediated degradable protein gel electrolyte according to claim 1, characterized in that: The specific steps are as follows: 1) Dissolve gelatin and sodium chloride in deionized water at a certain mass ratio, and stir at a constant temperature to obtain a transparent mixed solution; 2) adding a certain concentration of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide aqueous solution to the mixed solution obtained in step 1) in proportion, and coating to obtain a gel electrolyte with a certain thickness; 3) Soaking the gel electrolyte obtained in step 2) in a solution containing a certain concentration of sodium chloride and phytic acid to obtain a phytic acid-mediated degradable protein gel electrolyte.

3. The method for preparing the phytic acid-mediated degradable protein gel electrolyte according to claim 2, characterized in that: In step 1), 0.4-0.6 g of gelatin and 0.23-1.75 g of sodium chloride are weighed and added into 4-6 mL of deionized water; the gelatin is industrial gelatin; and in step 1), magnetic stirring is performed at 50-65° C. until the gelatin is dissolved into a transparent solution.

4. The method for preparing the phytic acid-mediated degradable protein gel electrolyte according to claim 2, characterized in that: In step 2), after the mixed solution obtained in step 1) is cooled to room temperature, 80 to 120 μL of 500 mg / mL 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide solution is added thereto while stirring, and the mixture is evenly dispersed; the evenly dispersed dispersion is coated on a polytetrafluoroethylene mold, allowed to stand at room temperature for 1 to 2 hours, and then removed from the polytetrafluoroethylene mold to obtain a complete gel sheet with a thickness of 0.8 to 1 cm.

5. The method for preparing the phytic acid-mediated degradable protein gel electrolyte according to claim 2, characterized in that: In the step 2), the uniformly dispersed dispersion is poured into a mold lined with polytetrafluoroethylene, and a cylindrical gel block is obtained by taking it out from the mold.

6. The method for preparing the phytic acid-mediated degradable protein gel electrolyte according to claim 2, characterized in that: In the step 3), 4.09-27.47 g of sodium chloride and 0.73-7.14 g of a phytic acid solution with a mass fraction of 70% are weighed, added to 100-200 mL of deionized water and mixed evenly to prepare a soaking solution for gel modification; then the gel electrolyte prepared in step 2) is soaked in the above-mentioned soaking solution for gel modification for 6-12 hours to obtain a phytic acid-mediated degradable protein gel electrolyte.

7. Use of the phytic acid-mediated degradable protein gel electrolyte according to claim 1 as a gel electrolyte for supercapacitors.

Citation Information

Patent Citations

  • Preparation method of gelatin-based gel electrolyte with double-network structure for metal fuel cell

    CN117487199A

Cited By

  • Protein gel as well as preparation method and application thereof

    CN121730401A