Sapphire substrate nitride semiconductor power device and manufacturing method thereof
By etching and depositing high thermal conductivity on the sapphire substrate, the low thermal conductivity and warping problems of nitride power devices of the sapphire substrate are solved, the heat dissipation and voltage resistance of the device are improved, and higher reliability is achieved and performance.
Patent Information
- Application Number
- CN202411000311.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
AI Technical Summary
Sapphire substrate nitride power devices have a problem of low thermal conductivity in high-power applications, which leads to an increase in chip temperature, affects reliability, and the prior art is difficult to effectively solve the problems of warpage and heat dissipation.
The substrate is completely or partially etched off on the sapphire substrate, and high thermal conductivity materials are deposited to improve the heat dissipation of the device, and improve crystal quality and pressure resistance by optimizing nucleation layer materials such as AlN, AlGaN, etc.
It improves the thermal conductivity and mechanical properties of the power chip, reduces the accuracy requirement for etching depth control, avoids etching damage to the nitride epitaxial layer, and achieves higher voltage withstandness and better device performance.
Smart Images

Figure CN118919558A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductors, and in particular relates to a nitride semiconductor power device on a sapphire substrate and a manufacturing method thereof. Background Art
[0002] Compared with traditional silicon devices, nitride semiconductor power devices are more energy-efficient, have more stable physical and chemical properties, can operate at higher ambient temperatures, have higher switching speeds, can reduce the volume and weight of application systems, and can be applied to a wide range of fields such as various household appliances, electric vehicles, solar and wind power generation, and large data centers. Gallium nitride is currently mainly used in the field of medium and low voltage consumer electronics. One of the reasons that limit its application in medium and high voltage is the high price of gallium nitride homogeneous substrates. In order to achieve higher cost-effectiveness, nitride epitaxial materials generally use heterogeneous epitaxy methods to grow nitride semiconductor materials on large-sized silicon substrates or sapphire substrates. The use of silicon substrates can utilize mature silicon semiconductor processing technology and equipment, and silicon substrates can be 8 inches or even 12 inches, which has obvious cost advantages compared to other types of substrates. However, at the interface between the silicon substrate and the nitride epitaxial layer, a conductive channel will be formed. Therefore, nitride semiconductor power devices based on silicon substrate epitaxy tend to break down first in the vertical direction under high voltage, and the withstand voltage of gallium nitride power devices is limited by the withstand voltage of the epitaxial material in the vertical direction. By increasing the thickness of the epitaxial material, the withstand voltage of the epitaxial material can be increased accordingly. However, due to the large mismatch between the silicon substrate and the nitride epitaxial material in terms of lattice size and thermal expansion coefficient, the thicker the epitaxial layer is, the greater the stress inside the epitaxial wafer is, which makes it difficult to control the stress and warping of the epitaxial wafer. At the same time, since the warping of the epitaxial wafer is also increased during the growth of the thick film, the growth conditions at different positions of the epitaxial wafer are more different, which reduces the uniformity of various parameters of the epitaxial wafer. The warping control problem and the uniformity problem of the epitaxial wafer will affect the yield and cost of the final product. In addition, the thicker the epitaxial material is grown, the longer the required growth time will be. Since the epitaxial production equipment is very expensive, this will also increase the cost of the product. The use of sapphire substrates to grow nitride epitaxy has been widely used in the production of nitride LEDs. It has the advantages of low cost and mature growth process. At the same time, unlike the conductive silicon substrate, the sapphire substrate is an insulating material with a high breakdown electric field. Therefore, by utilizing the withstand voltage of the sapphire substrate, it is not necessary to grow a thick nitride epitaxial layer, and the high withstand voltage of the chip can be achieved. One of the main problems limiting the application of nitride epitaxy on sapphire substrates in power devices is its low thermal conductivity. During the operation of the power device, heat cannot be effectively dissipated, causing the chip temperature to rise and affecting the chip reliability. Therefore, existing nitride power devices on sapphire substrates are generally limited to some low-power applications.
[0003] The invention patent with the patent number "CN116544194A" discloses a gallium nitride power device epitaxial wafer and its manufacturing method. A stress control layer is prefabricated on the back of the sapphire substrate to improve its warping problem, but its heat dissipation problem is not solved.
[0004] The invention patent with patent number "CN115346872A" discloses a chip manufacturing method for nitride semiconductor power devices. This method is for semiconductor devices on silicon substrates, and is mainly a replacement solution for the deficiencies in the existing technology of silicon substrate nitride epitaxial pressure resistance and heat dissipation.
[0005] The invention patent with the patent number of "CN117790439A" discloses a high-reliability sapphire substrate GaN power device and its preparation method. The scheme discloses etching a heat dissipation port under the sapphire substrate, depositing an AlN layer in the heat dissipation port, and depositing a back field plate metal layer on the side of the sapphire substrate away from the GaN high-resistance buffer layer, thereby solving the problem of poor heat dissipation capacity of the sapphire substrate GaN power device. However, this scheme requires the sapphire substrate to be completely etched away, the deposited insulating material is AlN, and the AlN layer deposited on the back is in contact with the high-resistance GaN layer of the epitaxial layer. In addition, dry etching of sapphire substrates generally uses Cl-containing gas, and wet etching of sapphire substrates generally uses high-temperature acidic solutions. These etching methods can also etch nitrides such as GaN, AlN, etc. Since the sapphire substrate to be etched is very thick and requires a very high etching rate, it is difficult to control the etching depth to stay at the interface between the nitride epitaxial layer and the sapphire substrate without causing obvious over-etching of the nitride epitaxial layer. Summary of the invention
[0006] In view of the problems in the background technology, especially the thermal conductivity problem of high electron mobility transistor (HEMT), the present invention provides a nitride semiconductor power device on a sapphire substrate, characterized in that it includes: a sapphire substrate, an epitaxial structure of a nitride semiconductor power device grown on the sapphire substrate, and a power device structure on the epitaxial structure, wherein the epitaxial structure at least includes: a nucleation layer on the substrate, and a nitride functional layer on the nucleation layer. A partial or complete etching area is provided at the position corresponding to the power device structure below the sapphire substrate, and a high thermal conductivity material is arranged at the etching area.
[0007] Optionally, for the sapphire substrate nitride semiconductor power device, if the sapphire substrate is completely etched away in the thickness direction perpendicular to the substrate surface, the nucleation layer does not include GaN single-layer material, and includes one of the following: AlN, AlGaN, AlGaInN, and a multilayer stack structure of the above materials; if part of the sapphire substrate is etched away in the thickness direction perpendicular to the substrate surface and part of the sapphire substrate is retained, the nucleation layer includes one of the following: GaN, AlN, AlGaN, AlGaInN, and a multilayer stack structure of the above materials.
[0008] Optionally, the power device at least includes a HEMT device structure, and the HEMT device structure includes: a source, a gate, and a drain, and may include depositing multiple layers of insulating dielectric materials.
[0009] Optionally, the functional layers of the epitaxial structure include: a buffer layer on the nucleation layer, a channel layer on the buffer layer, and a barrier layer on the channel layer.
[0010] Optionally, the etched area at least includes the entire area below the corresponding source and drain, and may also extend beyond the source and drain.
[0011] Optionally, the high thermal conductivity material includes at least one of the following: metal materials, metal alloy materials, non-metallic materials, and multilayer composite materials of the above materials. The metal materials include: Cu, Ag, Au, Al, Ni, and the non-metallic materials include: AlN, graphene.
[0012] Optionally, one or more insulating material layers are included above the high thermal conductivity material.
[0013] Optionally, when the high thermal conductivity material is a multi-layer composite material, one or more insulating material layers are inserted between the multi-layer composite materials.
[0014] Optionally, the buffer layer includes one of the following: AlN, AlGaN, a GaN single layer or multi-layer stacked structure, AlN / GaN, AlN / AlGaN, AlGaN / GaN super lattice structure, or a combination of the above structures.
[0015] Optionally, the channel layer includes one of the following materials: GaN material, AlGaN, and InGaN material.
[0016] Optionally, the barrier layer includes one of the following: an AlGaN layer, an AlN layer, an AlInN layer, AlInGaN, or a plurality of superpositions of the above material layers.
[0017] Optionally, an AlN insertion layer is further included between the channel layer and the barrier layer.
[0018] Optionally, the barrier layer further includes an unintentionally doped GaN cap layer or an in-situ SiN dielectric layer, or an alloy layer of p-type AlGaInN in any proportion.
[0019] The present invention also provides a method for preparing a nitride semiconductor epitaxial device on a sapphire substrate, which is at least used to manufacture the nitride semiconductor epitaxial device on a sapphire substrate as described in claim 1, comprising the following steps: S1, growing an epitaxial structure of a nitride semiconductor power device on a sapphire substrate; S2, manufacturing a power device structure above the epitaxial structure; S3, completely etching away the portion of the sapphire substrate below the corresponding device in a thickness direction perpendicular to the sapphire substrate, or etching away part of the substrate thickness to leave part of the sapphire substrate; S4, then depositing a high thermal conductivity material.
[0020] Optionally, the high thermal conductivity material is disposed in the etched area by electroplating, physical or chemical vapor deposition, or mechanical lift-off transfer.
[0021] Compared with the prior art, the present invention provides a sapphire substrate nitride semiconductor power device and a manufacturing method thereof, which has the following beneficial effects:
[0022] By using a sapphire substrate, the portion of the sapphire substrate below the corresponding device is completely etched in the direction perpendicular to the thickness of the sapphire substrate, or most of the substrate thickness is etched, leaving only part of the sapphire substrate, and then a material with good thermal conductivity is deposited to improve the thermal conductivity of the power chip. This solution can partially etch the sapphire substrate, which maintains better mechanical strength of the substrate than completely etching the sapphire substrate, eliminates the step of depositing AlN insulating material, and deposits high thermal conductivity materials to achieve better heat dissipation, while reducing the control accuracy requirements for the etching depth and causing no etching damage to the nitride epitaxial layer. This solution can also completely etch the sapphire substrate layer, but the nucleation layer of the nitride epitaxy on the sapphire does not use gallium nitride, but uses AlN, or AlGaN or AlGaInN alloy layer or a multilayer stack of the above materials. The optimized AlN nucleation layer can achieve better crystal quality than GaN materials, as well as better device horizontal withstand voltage. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Schematic diagram of the structure of the transistor of Example 1.
[0024] Figure 2a to Figure 2e A flow chart for transistor production of Example 1.
[0025] Figure 3 Schematic diagram of the structure of the transistor of Example 2.
[0026] Figures 4a to 4e A flow chart for transistor production of Example 2.
[0027] Among them: 11-sapphire substrate; 12-nucleation layer; 131-buffer layer; 132-channel layer; 133-barrier layer; 141-source; 142-gate; 143-drain; 15-insulating material layer; 16-high thermal conductivity material layer 16; 21-substrate; 22-nucleation layer; 231-buffer layer; 232-channel layer; 233-barrier layer; 241-source; 242-gate; 243-drain; 25-insulating material layer; 26-high thermal conductivity material layer. DETAILED DESCRIPTION
[0028] The present disclosure will now be described more fully below with reference to the accompanying drawings, however, the present disclosure can be implemented in many different ways and should not be construed as being limited to the embodiments set forth herein. On the contrary, providing these embodiments herein will make the present disclosure more detailed and complete, and fully convey the scope of the present disclosure to those skilled in the art. The same reference numerals throughout the text represent the same objects.
[0029] Example 1
[0030] In the first exemplary embodiment, referring to Figure 1 The structure of a nitride semiconductor power device on a sapphire substrate provided in this embodiment includes: a sapphire substrate 11, and a nucleation layer 12, a buffer layer 131, a channel layer 132, and a barrier layer 133 formed on the substrate 11 in sequence, and electrodes are formed on the barrier layer, including a source 141, a gate 142, and a drain 143. All sapphire substrate materials corresponding to the area between the source 141 and the drain 143, including the area directly below the source and the drain, are completely etched away, and then an insulating material layer 15 with good thermal conductivity is fully formed on the back. Then, a high thermal conductivity material layer 16 is formed.
[0031] In an optional embodiment, the substrate 11 is a sapphire substrate, and the nucleation layer is an AlN layer with a thickness of 0.5-200 nm. However, the embodiments of the present disclosure are not limited thereto, and the nucleation layer can also be AlGaN, or AlGaInN alloy material, or a multilayer stacked structure of the above materials.
[0032] In an optional embodiment, the buffer layer 131 is AlN with a thickness of 0.05-7 microns. However, the embodiments of the present disclosure are not limited thereto, and the buffer layer 131 may also be AlGaN, a GaN multilayer stacked structure, AlN / GaN, AlN / AlGaN, AlGaN / GaN superlattice structure, or a combination of the above structures.
[0033] In an optional embodiment, the channel layer 132 is made of GaN material with a thickness of 50-1000 nm. However, the embodiments of the present disclosure are not limited thereto. The channel layer 132 may also be made of AlGaN or InGaN material.
[0034] In an optional embodiment, the barrier layer 133 is an AlGaN layer with a thickness of 1-30 nm. However, the embodiments of the present disclosure are not limited thereto, and the barrier layer 133 may also be a plural superposition of 133AlN layer, AlInN layer, AlInGaN, or the above material layers.
[0035] In an optional embodiment, an AlN insertion layer may or may not be included under the barrier layer, and the thickness is 0.1-2 nm.
[0036] In an optional embodiment, a 0.1-10 nm GaN cap layer or a 0.5-150 nm in-situ SiN dielectric layer may or may not be included on the barrier layer.
[0037] In an optional embodiment, the source 141 , the gate 142 , and the drain 143 are made of metal.
[0038] Reference Figure 2a-2e As shown, this embodiment provides a method for manufacturing the sapphire substrate nitride semiconductor power device.
[0039] Step 1, such as Figure 2a As shown, a sapphire substrate 11 is provided, on which a nucleation layer 12, a buffer layer 131, a channel layer 132, and a barrier layer 133 are sequentially grown. The growth process is metal organic chemical vapor deposition (MOCVD) or molecular beam epitaxy (MBE), and other epitaxial technologies may also be used.
[0040] Step 2, such as Figure 2b As shown, a source 141, a gate 142 and a drain 143 are made on the upper surface of the epitaxial material. The above-mentioned electrode materials are generally metals, but can also be conductive non-metallic materials. The source and drain are ohmic contact electrodes, and the gate is a Schottky contact electrode. When making the source 141 and the drain 143, the barrier layer can be partially etched first to improve the ohmic contact characteristics and reduce the contact resistance, but it can also not be etched. When making the gate 142, depending on the different device technology routes, it is possible that the metal electrode is in direct contact with the barrier layer 133 to form a Schottky contact. It is also possible that there is a SiN or other insulating dielectric layer above the barrier layer, and the metal electrode is made on the insulating dielectric layer. In addition, if it is an enhanced device made using a p-type GaN cap layer, there is a 50-200nm p-type GaN cap layer above the barrier layer. At this time, the gate electrode 142 is made above the p-type GaN, which can be an ohmic contact or a Schottky contact.
[0041] Step 3, such as Figure 2cAs shown, all sapphire substrate materials in the area corresponding to the source 141 and the drain 143, including the area directly below the source and the drain, are completely etched away. The sapphire material is completely etched away in the vertical thickness direction to expose the nitride epitaxial material on the back. The etched area includes the effective area of the device below and between the source and the gate, and can be further extended to the area around the chip. Because it is not a partial area such as etching between the gate and the drain, but a large area of overall etching, it does not require a high etching selectivity ratio, nor does it require very precise alignment. Before etching, the thickness of the sapphire substrate is thinned to about 150 microns through a substrate thinning process to reduce the subsequent etching time. The etching method can be dry-etched using Cl-containing gases such as Cl2, BCl3, etc., and different etching rates can be used in stages. The early etching rate can reach 300nm / min or even higher. When etching to a lower residual substrate thickness, it is changed to a low etching rate to control the etching depth and reduce over-etching of the nitride epitaxial material.
[0042] Step 4, such as Figure 2d As shown, after etching is completed, an insulating material layer with good thermal conductivity is deposited on the back of the epitaxial wafer to improve the heat dissipation and voltage resistance of the chip. In this embodiment, the deposited material can be AlN or other insulating material layers. The deposition method can be physical vapor deposition such as sputtering, or chemical vapor deposition method, such as plasma enhanced chemical vapor deposition. The thickness can be 0.001-200 microns. This embodiment uses physical sputtering to deposit 5 microns of AlN material.
[0043] Step 5, such as Figure 2e As shown, high thermal conductivity materials are continuously deposited on the back of the epitaxial wafer to further improve the heat dissipation of the chip and the mechanical properties of the epitaxial wafer. The deposited material can be a metal material such as Cu, Ag, Au, etc., or other non-metallic materials with high thermal conductivity, such as graphene; or a combination of high thermal conductivity materials. Electroplating or physical, chemical deposition methods, or other methods such as mechanical stripping transfer method, bonding thermal conductive substrate method, etc. can be used, and the thickness can be 0.01-2000 microns. This embodiment uses electroplating to deposit 200 microns of Cu metal on the back of the epitaxial wafer.
[0044] Example 2
[0045] In the second exemplary embodiment, referring to Figure 3The structure of a nitride semiconductor power device on a sapphire substrate provided in this embodiment includes: a substrate 21, and a nucleation layer 22, a buffer layer 231, a channel layer 232, and a barrier layer 233 formed on the substrate 21 in sequence, and electrodes are formed on the barrier layer, including a source 241, a gate 242, and a drain 243. The sapphire substrate material corresponding to the source 241 and the drain 243, including the area directly below the source and the drain, is partially etched away, leaving an extremely thin sapphire substrate thickness, and then an insulating material layer 25 with good thermal conductivity is formed on the back side. Then, a high thermal conductivity material layer 26 is formed.
[0046] In an optional embodiment, the substrate 21 is a sapphire material substrate. The nucleation layer is an AlN layer with a thickness of 0.5-200 nm. However, the embodiments of the present disclosure are not limited thereto, and the nucleation layer can also be gallium nitride, indium nitride, or an alloy material of gallium nitride, indium nitride, and aluminum nitride in any proportion, or a multilayer stacked structure of the above materials.
[0047] In an optional embodiment, the buffer layer 231 is AlN with a thickness of 0.05-7 microns. However, the embodiments of the present disclosure are not limited thereto, and the buffer layer 231 may also be AlGaN, a GaN multilayer stacked structure, AlN / GaN, AlN / AlGaN, AlGaN / GaN superlattice structure, or a combination of the above structures.
[0048] In an optional embodiment, the channel layer 232 is made of GaN material with a thickness of 50-1000 nm. However, the embodiments of the present disclosure are not limited thereto, and the channel layer 232 may also be made of AlGaN or InGaN material.
[0049] In an optional embodiment, the barrier layer 233 is an AlGaN layer with a thickness of 1-30 nm. However, the embodiments of the present disclosure are not limited thereto, and the barrier layer 233 may also be an AlN layer, AlInN, AlInGaN, or a plurality of superpositions of the above material layers.
[0050] In an optional embodiment, an AlN insertion layer may or may not be included under the barrier layer, and the thickness is 0.1-2 nm.
[0051] In an optional embodiment, a 0.1-10 nm GaN cap layer or a 0.5-150 nm in-situ SiN dielectric layer may or may not be included on the barrier layer.
[0052] In an optional embodiment, the source 241 , the gate 242 , and the drain 243 are made of metal.
[0053] Reference Figure 4a-4e As shown, this embodiment provides a method for manufacturing a nitride semiconductor power device on a sapphire substrate.
[0054] Step 1, such as Figure 4a As shown, a sapphire substrate 21 is provided, on which a nucleation layer 22, a buffer layer 231, a channel layer 232, and a barrier layer 233 are sequentially grown. The growth process is metal organic chemical vapor deposition (MOCVD) or molecular beam epitaxy (MBE), and other epitaxial technologies may also be used.
[0055] Step 2, such as Figure 4b As shown, a source 241, a gate 242 and a drain 243 are made on the upper surface of the epitaxial material. The above-mentioned electrode materials are generally metals, but can also be conductive non-metallic materials. The source and drain are ohmic contact electrodes, and the gate is a Schottky contact electrode. When making the source 241 and the drain 243, the barrier layer can be partially etched first to improve the ohmic contact characteristics and reduce the contact resistance, but it can also not be etched. When making the gate 242, depending on the different device technology routes, it is possible that the metal electrode is in direct contact with the barrier layer 133 to form a Schottky contact. It is also possible that there is an in-situ SiN or other insulating dielectric layer above the barrier layer, and the metal electrode is made on the insulating dielectric layer. In addition, if it is an enhanced device made using a p-type GaN cap layer, there is a 1-300nm p-type GaN cap layer above the barrier layer. At this time, the gate electrode 242 is made above the p-type GaN, which can be an ohmic contact or a Schottky contact.
[0056] Step 3, such as Figure 4c As shown, part of the area corresponding to the source 241 and the drain 243 is etched away. In this embodiment, the remaining thickness of the sapphire substrate in the vertical thickness direction is 5 microns. The etching area of the sapphire substrate includes all areas directly below and between the source and the gate, and can be further extended to the surroundings of the area. Because it is not a partial area such as etching between the gate and the drain, but a large area of overall etching, it does not require a very high etching selectivity ratio, nor does it require very precise alignment. Before etching, the thickness of the sapphire substrate is thinned to 150 microns through a substrate thinning process to reduce the subsequent etching time. The etching method can use Cl-containing gases such as Cl2, BCl3, etc. for dry etching, and different etching rates can be used in stages. The early etching rate can reach 300nm / min or even higher. When etching to a lower residual substrate thickness, it is changed to a low etching rate to control the etching depth.
[0057] Step 4, such as Figure 4dAs shown, after etching is completed, an insulating material layer with good thermal conductivity is deposited on the back of the epitaxial wafer to improve the heat dissipation and voltage resistance of the chip. In this embodiment, the deposited material can be AlN or other insulating material layers. The deposition method can be physical vapor deposition such as sputtering, or chemical vapor deposition method, such as plasma enhanced chemical vapor deposition. The thickness can be 0.001-200 microns. In this embodiment, since the remaining unetched sapphire substrate has a thickness of 5 microns, it can be used to enhance the voltage resistance of the chip, so the deposition of the insulating material layer in this step can also be omitted. This embodiment uses physical sputtering to deposit 3 microns of AlN material with good thermal conductivity and insulation.
[0058] Step 5, such as Figure 4e As shown, high thermal conductivity materials are continuously deposited on the back of the epitaxial wafer to further improve the heat dissipation of the chip and the mechanical properties of the epitaxial wafer. The deposited material can be a metal material such as Cu, Ag, Au, etc., or other non-metallic materials with high thermal conductivity, such as AlN, graphene; or a combination of the above high thermal conductivity materials. Electroplating or physical, chemical vapor deposition methods, or other methods such as mechanical stripping transfer method, bonding thermal conductive substrate method, etc. can be used, and the thickness can be 0.01-2000 microns. This embodiment uses electroplating to deposit 200 microns of Cu metal on the back of the epitaxial wafer.
[0059] The above is only a specific implementation of the embodiment of the present invention, but the protection scope of the embodiment of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the embodiment of the present invention, which should be included in the protection scope of the embodiment of the present invention. Therefore, the protection scope of the embodiment of the present invention should be based on the protection scope of the claims.
Claims
1. A sapphire substrate nitride semiconductor power device, characterized in that: include: A sapphire substrate, an epitaxial structure of a nitride semiconductor power device grown on the sapphire substrate, and a power device structure on the epitaxial structure, wherein the epitaxial structure comprises at least: a nucleation layer on the substrate, a nitride functional layer on the nucleation layer, and a partial or complete etching area is provided at a position corresponding to the power device structure below the sapphire substrate, and a high thermal conductivity material is arranged at the etching area.
2. A sapphire substrate nitride semiconductor power device as claimed in claim 1, characterized in that: The etched area has a depth of completely etching away the sapphire substrate, and the nucleation layer includes one of the following: AlN, AlGaN, AlGaInN, and a multilayer stacked structure of the above materials.
3. The sapphire substrate nitride semiconductor power device according to claim 1, characterized in that: The depth of the etched area is such that most of the substrate thickness is etched away, leaving only a portion of the sapphire substrate, and the nucleation layer includes one of the following: GaN, AlN, AlGaN, AlGaInN, and a multilayer stacked structure of the above materials.
4. The sapphire substrate nitride semiconductor power device according to claim 1, characterized in that: The power device at least includes a HEMT device structure, and the HEMT device structure includes: a source, a gate, and a drain, and may include depositing multiple layers of insulating dielectric materials.
5. The sapphire substrate nitride semiconductor power device according to claim 1, characterized in that: The functional layers of the epitaxial structure include: a buffer layer on the nucleation layer, a channel layer on the buffer layer, and a barrier layer on the channel layer.
6. The sapphire substrate nitride semiconductor epitaxial device according to claim 1, characterized in that: The etched area at least includes the entire area below the corresponding source and drain, and may also extend beyond the source and drain.
7. The sapphire substrate nitride semiconductor epitaxial device according to claim 1, characterized in that: The high thermal conductivity material includes at least one of the following: metal material, metal alloy material, non-metal material, and multilayer composite material of the above materials. The metal material includes: Cu, Ag, Au, Al, Ni, and the non-metal material includes: AlN, graphene.
8. The sapphire substrate nitride semiconductor epitaxial device according to claim 1, characterized in that: One or more insulating material layers are also included above the high thermal conductivity material.
9. The sapphire substrate nitride semiconductor epitaxial device according to claim 6, characterized in that: When the high thermal conductivity material adopts a multi-layer composite material, one or more insulating material layers are inserted between the multi-layer composite material layers.
10. A method for preparing a nitride semiconductor epitaxial device on a sapphire substrate, at least for preparing the nitride semiconductor epitaxial device on a sapphire substrate as claimed in claim 1, comprising the following steps: S1. Growing an epitaxial structure of a nitride semiconductor power device on a sapphire substrate; S2, fabricating a power device structure on top of the epitaxial structure; S3, completely etching away the portion of the sapphire substrate below the corresponding device in a direction perpendicular to the thickness of the sapphire substrate, or etching away part of the thickness of the substrate to leave part of the sapphire substrate; S4. Depositing high thermal conductivity material.
11. The method for preparing a nitride semiconductor epitaxial device on a sapphire substrate according to claim 9, characterized in that: The high thermal conductivity material is deposited on the etched area by electroplating, physical or chemical vapor deposition, or mechanical lift-off transfer.