Pre-sodium-modified hard carbon negative electrode, pre-sodium-modified method and application
By pre-sodiumization of 9-fluorenone sodium solution on the hard carbon negative electrode of sodium ion battery, the problem of low Coulomb efficiency for the first time was solved, the battery energy density was improved and process simplified was achieved, and the commercial development of sodium ion battery was provided. New ideas.
Patent Information
- Application Number
- CN202410826521.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-11-08
AI Technical Summary
The first time during the charging and discharging process of sodium ion battery, the Coulombic efficiency is low and the circulation performance is poor, mainly due to the irreversible reaction and the irreversible loss of sodium, resulting in battery energy loss.
The hard carbon negative electrode was pre-sodiumed by spraying the 9-fluorenone sodium solution on the surface of the hard carbon negative electrode, combining tetrahydrofuran or ethylene glycol dimethyl ether as solvent, and using corn starch and potato starch As a hard carbon precursor, the pre-sodium hardened carbon negative electrode was prepared by room temperature reaction and subsequent washing and drying.
It significantly improves the first Coulomb efficiency of hard carbon negative electrodes, reduces battery energy loss caused by irreversible consumption, simplifies the process flow, makes it easier to industrialize and promote, and improves the performance of sodium ion batteries.
Smart Images

Figure CN118919882A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of batteries, in particular to a pre-sodiumized hard carbon negative electrode, a pre-sodiumization method of the pre-sodiumized hard carbon negative electrode, and application of a pre-sodiumization reagent in the pre-sodiumized hard carbon negative electrode. Background Art
[0002] Lithium-ion batteries have been widely studied due to their excellent electrochemical properties. However, with the advent of the era of electric vehicles and smart grids, the shortage of lithium resources will become an important factor restricting their development. It is well known that the reserves of metallic sodium are relatively abundant in the earth's crust. The sodium content in the earth's crust is about 2.75%, while the lithium content is about 0.065‰. In addition, the distribution area is wide. Sodium is distributed all over the world, while about 70% of lithium is concentrated in South America. At the same time, sodium and lithium have similar physical and chemical properties and similar extraction / embedding mechanisms. Therefore, the research and development of sodium-ion batteries is expected to alleviate the problem of limited development of energy storage batteries caused by the shortage of lithium resources to a certain extent.
[0003] As the most promising negative electrode material for sodium-ion batteries, hard carbon materials still face problems such as low initial coulombic efficiency and poor cycle performance during the charge and discharge process. On the one hand, the electrolyte decomposes to form a solid electrolyte phase (SEI) during the cycle, consuming part of the sodium source; on the other hand, irreversible reactions caused by high specific surface area, pores, defects and functional groups will also cause irreversible loss of sodium. Traditionally, methods such as reducing the specific surface area of hard carbon materials, regulating defect types, regulating the size and proportion of nanopores, and optimizing electrolyte components can improve the initial efficiency to a certain extent, but problems such as process complexity and cost controllability mean that it is still some distance away from commercialization. Summary of the invention
[0004] The present invention aims to solve the problem of low initial coulombic efficiency of hard carbon negative electrode materials for sodium ion batteries in the prior art, and provides a pre-sodiumized hard carbon negative electrode, a pre-sodiumization method and an application thereof. The specific technical scheme is as follows:
[0005] In a first aspect, the present application provides a pre-sodiumized hard carbon negative electrode, wherein a pre-sodiumization reagent is sprayed on the surface of the hard carbon negative electrode, and the pre-sodiumization reagent is a 9-fluorenone sodium solution.
[0006] As a further technical solution of the present invention, the concentration of the 9-fluorenone sodium solution is 0.01-1 mol·L -1 .
[0007] As a further technical solution of the present invention, the solvent of the pre-sodium reagent solution is tetrahydrofuran or ethylene glycol dimethyl ether.
[0008] As a further technical solution of the present invention, the spraying surface density is 0.5L·m -2 .
[0009] As a further technical solution of the present invention, the hard carbon negative electrode precursor is one or more of corn starch, potato starch, and sweet potato starch.
[0010] In a second aspect, the present application provides a pre-sodiumization method for a pre-sodiumized hard carbon negative electrode, and the specific steps are as follows:
[0011] S1, preparation of hard carbon negative electrode;
[0012] S2, presodiumization;
[0013] 9-fluorenone is dissolved in tetrahydrofuran solvent, and then sodium is finally added thereto. After the reaction is completed at room temperature, a tetrahydrofuran solution of 9-fluorenone sodium is obtained. A pre-sodiumization reagent is sprayed on the surface of the hard carbon negative electrode of the sodium ion battery. After the reaction is complete, the hard carbon negative electrode of the sodium ion battery is washed and dried to obtain a pre-sodiumized hard carbon negative electrode.
[0014] As a further technical solution of the present invention, the dissolution conditions of 9-fluorenone in S2 are dew point ≤ -40°C and temperature 25°C.
[0015] As a further technical solution of the present invention, the steps for preparing the hard carbon negative electrode of S1 are as follows:
[0016] S11, sintering the starch in an air atmosphere at 210°C for 2-8h, crushing the sintered sample with a crusher, and finally pyrolyzing at 1100-1500°C for 1-6h to finally obtain hard carbon powder;
[0017] S12, hard carbon powder, conductive agent and binder are mixed in proportion, deionized water is used as solvent, and after high-speed stirring for 12 hours, the obtained slurry is applied to the surface of aluminum foil, and vacuum dried at 80°C for 12 hours for standby use, thereby obtaining a corn starch-based hard carbon negative electrode.
[0018] As a further technical solution of the present invention, the heating rate in S11 is 5°C·min -1 .
[0019] On the third aspect, the present application also provides the application of pre-sodiumized hard carbon negative electrode in the field of sodium ion batteries.
[0020] The beneficial effects of the present invention are as follows:
[0021] (1) In the present application, a sodium 9-fluorenone solution is used to react with a hard carbon negative electrode to obtain a pre-sodiumized hard carbon negative electrode, which effectively improves the first coulombic efficiency and avoids battery energy loss due to irreversible consumption.
[0022] (2) The pre-sodiumization method in the present application has simple steps and significant effects. It effectively improves the initial coulombic efficiency and avoids battery energy loss due to irreversible consumption. It is easy to promote industrialization and opens up new ideas for the development of sodium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The first week charge and discharge curves of the hard carbon negative electrode material before and after pre-sodiumization obtained in Example 1 are shown;
[0024] Figure 2 The first week charge and discharge curves of the hard carbon negative electrode material before and after pre-sodiumization obtained in Example 2 are shown. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments.
[0026] Example 1
[0027] Weigh 2.5 g corn starch and sinter it at 210 °C in air for 6 h, with a heating rate of 5 °C min -1 The sintered samples were crushed with a crusher and finally pyrolyzed at 1400 °C for 3 h with a heating rate of 5 °C min -1 , and finally obtain hard carbon powder.
[0028] Take 80 parts of hard carbon powder, 10 parts of conductive agent and 10 parts of CMC binder by mass, use deionized water as solvent, stir at high speed for 12 hours, apply the obtained slurry to the surface of aluminum foil, and dry it in vacuum at 80°C for 12 hours before use to obtain a corn starch-based hard carbon negative electrode.
[0029] Under the conditions of dew point ≤ -40℃ and temperature 25℃, 1.8g of 9-fluorenone was dissolved in 20mL of tetrahydrofuran solvent, and then 0.23g of sodium was finally added to it. After the reaction was completed at room temperature, the concentration was 0.5mol·L -1 A tetrahydrofuran solution of sodium 9-fluorenone is prepared, and the pre-sodiumization reagent is sprayed on the surface of the hard carbon negative electrode of the sodium ion battery. After the reaction is complete, the hard carbon negative electrode of the sodium ion battery is washed and dried to obtain the pre-sodiumized hard carbon negative electrode.
[0030] At room temperature, constant current charge and discharge tests were performed using the NEWAREC-3008 battery test system. Figure 1 As shown, the test voltage range is 0.01-2.5V, and the current density is 30mA·g -1 , Figure 1The results show that after pre-sodiumization, the open circuit voltage of the half-cell decreased from 2.567V to 0.761V, indicating the successful realization of pre-sodiumization. As can be seen from the figure, the first discharge capacity of the hard carbon negative electrode is 362.93mAh·g -1 The first charge capacity is 280.85 mAh g -1 , while the first discharge capacity of the pre-sodiumized hard carbon anode is 304.37 mAh g -1 The first charge capacity is 303.48 mAh g -1 Compared with the non-pre-sodiumized hard carbon electrode, the first coulombic efficiency of the pre-sodiumized electrode was significantly improved, from 77.38% to 99.71%.
[0031] Example 2
[0032] Weigh 2.5 g of sweet potato starch and sinter it in air at 250 °C for 2 h, with a heating rate of 5 °C min -1 The sintered samples were crushed with a crusher and finally pyrolyzed at 1400 °C for 2 h, with a heating rate of 5 °C min -1 , and finally obtain hard carbon powder.
[0033] Take 80 parts of hard carbon powder, 10 parts of conductive agent and 10 parts of PVDF binder by mass, use N-methylpyrrolidone as solvent, stir at high speed for 12 hours, apply the obtained slurry to the surface of aluminum foil, and dry it in vacuum at 80°C for 12 hours before use to obtain a sweet potato starch-based hard carbon negative electrode.
[0034] Under the conditions of dew point ≤ -40℃ and temperature 25℃, 1.8g of 9-fluorenone was dissolved in 10mL of tetrahydrofuran solvent, and then 0.23g of sodium was finally added to it. After the reaction was completed at room temperature, the concentration was 1mol·L -1 A tetrahydrofuran solution of sodium 9-fluorenone is prepared, and the pre-sodiumization reagent is sprayed on the surface of the hard carbon negative electrode of the sodium ion battery. After the reaction is complete, the hard carbon negative electrode of the sodium ion battery is washed and dried to obtain the pre-sodiumized hard carbon negative electrode.
[0035] At room temperature, constant current charge and discharge tests were performed using the NEWAREC-3008 battery test system. Figure 1 As shown, the test voltage range is 0.01-2.5V, and the current density is 30mA·g -1 , Figure 2 The results show that after pre-sodiumization, the open circuit voltage of the half-cell decreased from 2.215V to 1.217V, indicating the successful realization of pre-sodiumization. As can be seen from the figure, the first discharge capacity of the hard carbon negative electrode is 537.17mAh·g -1 The first charge capacity is 352.39 mAh g -1, while the first discharge capacity of the pre-sodiumized hard carbon anode is 345.84 mAh g -1 The first charge capacity is 345.39 mAh g -1 Compared with the non-pre-sodiumized hard carbon electrode, the first coulombic efficiency of the pre-sodiumized electrode was significantly improved, from 65.67% to 99.87%.
[0036] In summary, the method of pre-sodiumizing the hard carbon negative electrode of sodium ion batteries using 9-fluorenone sodium reagent has significant effects, simple process, and is easy to promote industrialization. The hard carbon negative electrode pre-sodiumized by this method is matched with the positive electrode material to obtain a sodium ion full battery with high first-week efficiency and high energy density, which has broad research prospects and application value.
[0037] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them.
Claims
1. A pre-sodiumized hard carbon negative electrode, characterized in that: The surface of the hard carbon negative electrode is sprayed with a pre-sodium reagent, and the pre-sodium reagent is a 9-fluorenone sodium solution.
2. The pre-sodiumized hard carbon negative electrode according to claim 1, characterized in that: The concentration of the 9-fluorenone sodium solution is 0.01-1 mol·L -1 .
3. The pre-sodiumized hard carbon negative electrode according to claim 2, characterized in that: The solvent of the pre-sodium reagent solution is tetrahydrofuran or ethylene glycol dimethyl ether.
4. The pre-sodiumized hard carbon negative electrode according to claim 1, characterized in that: The spraying surface density is 0.5L·m -2 .
5. The pre-sodiumized hard carbon negative electrode according to claim 4, characterized in that The hard carbon negative electrode precursor is one or more of corn starch, potato starch and sweet potato starch.
6. The method for pre-sodiumization of a pre-sodiumized hard carbon negative electrode according to any one of claims 1 to 5, characterized in that: The specific steps are as follows: S1, preparation of hard carbon negative electrode; S2, presodiumization; 9-fluorenone is dissolved in tetrahydrofuran solvent, and then sodium is finally added thereto. After the reaction is completed at room temperature, a tetrahydrofuran solution of 9-fluorenone sodium is obtained. A pre-sodiumization reagent is sprayed on the surface of the hard carbon negative electrode of the sodium ion battery. After the reaction is complete, the hard carbon negative electrode of the sodium ion battery is washed and dried to obtain a pre-sodiumized hard carbon negative electrode.
7. The method for pre-sodiumization of a pre-sodiumized hard carbon negative electrode according to claim 6, characterized in that: The dissolution conditions of 9-fluorenone in S2 are dew point ≤ -40°C and temperature 25°C.
8. The method for pre-sodiumization of a pre-sodiumized hard carbon negative electrode according to claim 6, characterized in that: The steps for preparing the hard carbon negative electrode of S1 are as follows: S11, sintering the starch in an air atmosphere at 210°C for 2-8h, crushing the sintered sample with a crusher, and finally pyrolyzing at 1100-1500°C for 1-6h to finally obtain hard carbon powder; S12, mix the hard carbon powder, conductive agent and binder in proportion, use ionized water as solvent, stir at high speed for 12 hours, apply the obtained slurry to the surface of aluminum foil, and vacuum dry it at 80°C for 12 hours for standby use, so as to obtain a corn starch-based hard carbon negative electrode.
9. The method for pre-sodiumization of a pre-sodiumized hard carbon negative electrode according to claim 6, characterized in that: The heating rate in S11 is 5°C·min -1 .
10. Application of the pre-sodiumized hard carbon negative electrode according to any one of claims 1 to 5 in the field of sodium ion batteries.