Waste battery material direct repair system based on redox targeting reaction and application of waste battery material direct repair system

Through the direct repair system of waste battery materials based on redox targeted reactions, the problems of high energy consumption and pollution in lithium-ion battery recycling are solved, low-cost and sustainable battery electrode material repair is achieved, and resource waste and environmental pollution are reduced. Suitable for industrial scale production.

CN118919906APending Publication Date: 2024-11-08SOUTH CHINA NORMAL UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410846115.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing lithium-ion battery recycling technology has high energy consumption, pollution and unsustainability, especially the high cost of recycling batteries without high economic value metals is high and profits cannot be covered, and there is waste of resources and environment for the management and resource recycling of used batteries. threaten.

Method used

The direct repair system of waste battery materials based on redox targeted reaction is adopted. Through the combination of the repair unit and the energy storage unit, the missing lithium ions are embedded back into the battery by using the redox reaction to realize the repair of the electrode material, and the water-based battery technology is used. It realizes ion compensation and recycling with the ion exchange membrane.

Benefits of technology

It realizes low-cost and sustainable battery electrode material repair, reduces greenhouse gas emissions and secondary pollution, improves recycling efficiency, is suitable for industrial-scale production, and has the advantages of environmentally friendly and economical benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919906A_ABST
    Figure CN118919906A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of novel energy material technology and waste battery material repairing, and discloses a waste battery material direct repairing system based on redox targeting reaction and application thereof. The system comprises a repairing unit and an energy storage unit, the energy level matching and ion compensation technology is adopted, an active material and an electrode material are subjected to a redox reaction, and missing lithium ions in a waste battery are directly embedded back; and then the device is integrated with an aqueous battery technology to form a multifunctional device, so that the purpose of sustainable compensation of target ions is achieved, and meanwhile, cyclic utilization of part of reactants in the device is promoted. The operation process of the electrochemical continuous repair electrode material is simple and convenient, the method has practical application value in the aspect of waste battery repair, and the method is suitable for large-scale production and use of factories; the method can be applied to the aspects of industrial waste treatment, waste battery repair, energy conversion and storage and other fields needing electric energy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of new energy material technology and waste battery material repair technology, and in particular relates to a waste battery material direct repair system based on redox targeted reaction and its application. Background Art

[0002] Lithium-ion batteries (LIBs) have become the main power source for electric vehicles due to their high energy density and good cycle performance. The growth of the electric vehicle market has stimulated the rapid development of the lithium-ion battery (LIBs) industry. The improvement of production efficiency and the further reduction of manufacturing costs have also promoted the widespread application of lithium-ion batteries in various industries. The life of power batteries is usually only 5 to 8 years. Even if cascade utilization is achieved, a large number of scrapped batteries will still be generated. It is estimated that by 2040, about 14 million LIBs will be generated each year. If not effectively treated, the harmful metals and other toxic substances in these waste batteries will pose a serious threat to the environment and human health, and will also cause waste of resources. With the expansion of the LIBs market, the effective recycling of LIBs has become an urgent problem to be solved.

[0003] From a resource perspective, key elements in LIBs, such as lithium, cobalt, and nickel, are unevenly distributed on the earth's crust, and continued mining has exacerbated the irreversible loss of natural resources. Due to the imbalance between supply and demand caused by the rapid development of batteries, the prices of metals such as cobalt, lithium, and nickel have continued to rise in the international market. Currently, 35% of global lithium production is used in LIBs, and by 2025, the demand for LIBs is expected to reach 66% (of lithium production). The metals (such as Co, Li, Cu, Al, Fe, and Ni) in waste LIBs are rich, and some even exceed the content in natural ores. Recycling these metals from waste LIBs can not only reduce dependence on upstream raw materials and ease resource tensions, but also bring economic benefits and reduce environmental pollution. Therefore, the proper management of waste LIBs and the growing demand for LIBs raw materials have spawned a huge waste LIBs recycling market.

[0004] Current battery recycling technologies generally have problems such as high energy consumption, high pollution and unsustainability. For example, the pyrometallurgical recycling process consumes a lot of energy and emits a lot of greenhouse gases. The wet recycling process consumes a lot of chemicals (acids, alkalis, precipitants) and will cause secondary pollution problems. However, for LIBs that do not contain metals of high economic value (such as LiFePO4), the profits generated by traditional recycling methods cannot make up for their high processing costs.

[0005] In summary, our research aims to promote the efficient recycling and restoration of spent LIBs and promote the sustainable development of the new energy industry. Summary of the invention

[0006] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a direct repair system for waste battery materials based on redox targeted reactions.

[0007] Another object of the present invention is to provide a method for directly repairing waste battery materials based on redox targeted reactions.

[0008] Another object of the present invention is to provide the application of the above-mentioned direct repair system for waste battery materials based on redox targeted reaction in the recovery and repair of waste battery materials.

[0009] The purpose of the present invention is achieved through the following solutions:

[0010] A direct repair system for waste battery materials based on redox targeted reaction, comprising a repair unit and an energy storage unit, wherein:

[0011] The repair unit is a liquid storage tank containing the battery electrode material to be repaired and a filter membrane; the filter membrane separates the liquid storage tank into two layers, and the battery electrode material to be repaired is placed in the lower layer; the filter membrane allows liquid to pass through, but will intercept solid particles, thereby realizing solid-liquid separation in the repair unit.

[0012] The energy storage unit is constructed based on an aqueous battery, which includes a positive electrode current collector, a positive electrode electrolyte, a lithium supply solution (or a sodium supply solution), a negative electrode electrolyte and a negative electrode current collector in sequence. Different solutions are divided into different chambers by ion exchange membranes to achieve different functions. The general structure is similar to "||positive electrode electrolyte||lithium supply solution (or sodium supply solution)||negative electrode electrolyte||"; the solutions in each chamber are circulated by a circulating pump.

[0013] The repair unit is connected to the positive electrolyte of the energy storage unit through a circulation pump and pipeline to form a cycle. That is, the positive electrolyte is pumped out from the energy storage unit, enters the lower layer of the repair unit, directly contacts and reacts with the battery electrode material to be repaired, and then is filtered through the filter membrane to achieve solid-liquid separation with the battery electrode material to be repaired, enters the upper layer of the repair unit, and finally flows back to the positive electrolyte of the energy storage unit.

[0014] The battery electrode material to be repaired can be a lithium battery or sodium battery material, such as LiFePO4, LiNiO2, LiCoO2, Na3MnTi(PO4)3, Na3V2(PO4)3, ternary NCA or NCM electrode materials (such as LiNi 1 / 3 Co 1 / 3 Al 1 / 3 O2、LiNi 1 / 3Co 1 / 3 Mn 1 / 3 O2、LiN i0.5 Co 0.3 Al0.2 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2、LiNi 0.6 Co 0.2 Al 0.2 O2、LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.8 Co 0.1 Al 0.1 O2, etc.), and modified versions of these materials. The electrode material is the main raw material for repairing the target element and is the key material for promoting the continuous operation of the present invention.

[0015] The filter membrane is at least one of glass fiber diaphragm, filter paper, nylon filter membrane, polytetrafluoroethylene filter membrane, mixed cellulose filter membrane, polyethersulfone filter membrane, polypropylene filter membrane and polyvinylidene fluoride filter membrane; the retention particle size of the filter membrane is 0.1 to 50 μm, and the retention particle size of the membrane is preferably ≤0.4 μm.

[0016] The positive electrode current collector is a conductive carrier; wherein the conductive carrier includes at least one of conductive carriers with a larger specific surface such as carbon cloth, hydrophobic carbon cloth, carbon paper, graphite paper, zinc sheet, aluminum foil, copper foil, foam metal, etc.

[0017] The negative electrode current collector is a negative electrode active material or a conductive carrier; the negative electrode active material includes one of active metal electrode materials such as Cu, Sn, Pb, Zn, Fe, Ga, and Mn; the conductive carrier includes at least one of conductive carriers with a larger specific gravity such as carbon cloth, hydrophobic carbon cloth, carbon paper, graphite paper, zinc sheet, aluminum foil, copper foil, and foam metal.

[0018] The positive electrode electrolyte is an aqueous solution containing positive electrode active materials, wherein the positive electrode active materials are materials with redox activity, including but not limited to ascorbic acid (Vc), citric acid, magnesium ascorbate, sodium ascorbate, [Fe(CN)6] 3- , [Fe(CN)6] 4- 、FeCl2、TEMPO、I - , BTMAP-Fc, FcNCl or FcN2Br2 and other active substances with redox function; the concentration of the positive electrode active substance in the positive electrode electrolyte is ≥10mM, and the pH range should be between 2-7. A pH buffer can also be added to the positive electrode electrolyte to stabilize its pH, and the pH buffer includes but is not limited to one of glycine-hydrochloric acid buffer, potassium dihydrogen phosphate-citric acid buffer, potassium dihydrogen phosphate-dipotassium hydrogen phosphate buffer and potassium hydrogen phthalate-potassium hydroxide buffer.

[0019] The positive electrode electrolyte may also include an auxiliary conductive additive. The type of the auxiliary conductive additive is determined by the goal of the direct repair system and is generally consistent with the anion supply of the lithium solution (or sodium solution) in the adjacent chamber.

[0020] When the negative electrode current collector is a negative electrode active material, the negative electrode electrolyte is water or an aqueous solution of a salt containing the corresponding negative electrode active material. For example, if the negative electrode current collector is Zn, the negative electrode electrolyte can be water or a Zn salt solution. At this time, the concentration of the salt solution of the negative electrode active material is ≥10mM.

[0021] When the negative electrode current collector is a conductive carrier, the negative electrode electrolyte is an aqueous solution of a negative electrode active material, wherein the negative electrode active material is V 2+ Cr 2+ 、Ti 3+ and I2, etc.

[0022] The negative electrode electrolyte may also include auxiliary conductive additives. The type of the auxiliary conductive additive is determined by the goal of the direct repair system, and generally maintains cation consistency with the negative electrode active material; and maintains anion consistency with the lithium supply solution (or sodium supply solution) in the adjacent chamber, including but not limited to ZnSO4, ZnCl2, FeSO4 and FeCl2.

[0023] The auxiliary conductive additives in the positive and negative electrolytes are relatively independent and include at least one of NaCl, NaF, Na2SO4, KCl, LiCl, LiF, Li2SO4, ZnSO4, ZnCl2, FeSO4 and FeCl2, CH3COOLi2 and LiNO3, etc., which are used to improve the conductivity of the solution. For the consistency of ions, the type of auxiliary conductive agent can be determined according to the type of anion or cation exchanged between the electrolyte and the adjacent chamber solution. The concentration of the auxiliary conductive agent in the positive and negative electrolytes is relatively independent and is 0M to 1M, preferably 0.1M to 1M.

[0024] The lithium supply solution is a solution containing lithium metal ions, preferably at least one of Li2SO4 solution, LiCl solution, LiF solution, LiNO3 solution, and CH3COOLi2 solution. The above lithium supply solutions can be reasonably matched according to different repair or collection purposes. The concentration of the lithium supply solution is relatively independent and is 0.1M to 3M, preferably 0.5M to 2M, and more preferably 1M to 1.5M.

[0025] The sodium supply solution is a solution containing sodium metal ions, preferably at least one of NaCl solution, Na2SO4 solution, NaNO3 solution, NaF solution, CH3COONa2 solution, etc. The above sodium supply solutions can be reasonably matched according to different repair or collection purposes. The concentration of the sodium supply solution is relatively independent and is 0.1M to 3M, preferably 0.5M to 2M, and more preferably 1M to 1.5M.

[0026] Preferably, when the battery electrode material to be repaired is waste LiFePO4, the positive electrode active material is at least one of ascorbic acid, citric acid, sodium ascorbate and magnesium ascorbate, and the concentration of the positive electrode active material in the positive electrode electrolyte is 30 to 100 mM;

[0027] Preferably, when the battery electrode material to be repaired is waste LiCoO2, the positive electrode active material is [Fe(CN)6] 3- , [Fe(CN)6] 4- , FeCl2, TEMPO, LiI, and the concentration of the positive electrode active material in the positive electrode electrolyte is 10 to 100 mM.

[0028] Preferably, when the battery electrode material to be repaired is waste LiNiO2, LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.8 Co 0.1 Al 0.1 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2、LiNi 0.6 Co 0.2 Al 0.2 O2、LiNi 0.5 Co 0.3 Mn 0.2 O2、LiN i0.5 Co 0.3 Al 0.2 O2、LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2、LiNi 1 / 3 Co 1 / 3 Al 1 / 3 When LiO2, LiTMO2 or LiTMPO4, the positive electrode active material is ascorbic acid, citric acid, sodium ascorbate, I - / I3 - At least one of the following; the concentration of the positive electrode active material in the positive electrode electrolyte is 20 to 100 mM;

[0029] Preferably, when the battery electrode material to be repaired is waste LiFePO4, the lithium supply solution is one of Li2SO4 solution and Li3PO4 solution.

[0030] The ion exchange membrane includes at least one of an anion exchange membrane (AEM) and a cation exchange membrane (CEM). The ion exchange membrane is placed between the electrolyte and the lithium supply solution (sodium supply solution) for ion exchange and isolation. Generally, the anion / cation exchange membranes are placed alternately.

[0031] The anion exchange membrane comprises an anion exchange membrane containing -NH2 (amino group), an anion exchange membrane containing -N(CH3)3OH (quaternary amine group), a chloride ion exchange membrane, a sulfate ion exchange membrane, and a nitrate ion exchange membrane, preferably an ion exchange membrane containing -N(CH3)3OH (quaternary amine group) and a chloride ion exchange membrane;

[0032] The cation exchange membrane includes a cation exchange membrane containing -SO3H (sulfonic acid group), a cation exchange membrane containing -COOH (carboxyl group), a fast ion conductor film, a sodium ion exchange membrane, a lithium ion exchange membrane, a potassium ion exchange membrane, a calcium ion exchange membrane and a magnesium ion exchange membrane; preferably, it is a cation exchange membrane containing -SO3H (sulfonic acid group) and a lithium ion exchange membrane (or a sodium ion exchange membrane).

[0033] The fast ion conductor film includes Si-OC, Si-OC-Al, Si-CN, Si-ON, Si-OCN, Si-C, Si-N and other systems, as well as Li 1+x Al x Ge 2-x( PO4)3(LAGP) and Li 1+x Al x Ti 2-x (PO4)3(LATP), Li7La3Zr2O 12 (LLZO), LiGeP2S 12 (LGPS), Na 1+x Zr2Si 2-x P x O 12 One of the fast ion conductor films, wherein 0≤x≤2; preferably Li 1+x Al x Ti 2-x (PO4)3 and Na 1+x Zr2Si 2-x P x O 12A type of membrane in a system. Fast ion conductor membranes have stronger ion selectivity and can only pass through a single ion. Generally, they have advantages when the ions that pass through the membrane are lithium ions or sodium ions.

[0034] A method for directly repairing waste battery materials based on redox targeted reaction, comprising the following steps:

[0035] (1) Preparing a positive electrode electrolyte, a negative electrode electrolyte and a lithium supply solution (or a sodium supply solution): the positive electrode active material, the negative electrode active material and the lithium supply material (or the sodium supply material) are uniformly dissolved in water to obtain a positive electrode electrolyte, a negative electrode electrolyte and a lithium supply solution (or a sodium supply solution);

[0036] (2) assembling a lithium supply solution (or sodium supply solution), a positive electrode electrolyte, a negative electrode electrolyte, a positive electrode current collector material, a negative electrode current collector material, and an ion exchange membrane into an aqueous battery device, i.e., an energy storage unit;

[0037] (3) The positive electrode electrolyte in the energy storage unit is pumped out, and after direct contact and reaction with the electrode material to be repaired in the repair unit, the solution and the electrode material to be repaired are separated by a filtration membrane and flowed back to the energy storage unit to promote the continuation of the repair reaction; the reaction of the repair process is: A+Li + +O=A n+ +R or A+Na + +O=A n+ +R; O is the positive electrode material to be repaired, and R is the repaired positive electrode material. After O is reduced by A, the valence state is reduced, and then Li in the lithium supply solution is obtained. + To achieve charge balance, thereby replenishing the missing Li; or to obtain Na in the sodium supply solution + , replenish the missing Na and complete the repair process;

[0038] (4) When the positive electrode electrolyte flows back from the repair unit, the energy storage unit circuit is closed. Due to the different potentials of the redox reactions at both ends, a potential difference is generated, which supplies power to the reduction active material and drives the repair reaction to proceed continuously. The reaction at the positive electrode is: A n+ +ne - =A; the reaction at the negative electrode is: B-ne - =B n+ ; Wherein A is the reduced state of the above-mentioned positive electrode active material, A n+ is the corresponding oxidation state; and B corresponds to the reduced state of the above-mentioned negative electrode active material, B n+ is the corresponding oxidation state.

[0039] For example, the material O to be repaired is Li 1-x FePO4 (i.e. waste LiFePO4, which is missing some Li +LiFePO4), the positive electrode active material A is Vc. Through the repair reaction, Vc converts Li 1-x After the Fe in FePO4 is reduced to a low valence state, the Li in the lithium supply solution is obtained. + And supplement the missing Li to generate LiFePO4 (ie R); at the same time, Vc 2+ (i.e. A n+ ) obtains electrons in the energy storage device and is reduced to A, ultimately achieving the recycling of A.

[0040] In order to evenly disperse the solute in water, step (1) is preferably performed by ultrasonication at 40 to 100 kHz for 0.5 to 1.5 hours.

[0041] When the positive electrode electrolyte and the negative electrode electrolyte described in step (1) further include auxiliary conductive additives, it is preferred that the positive electrode active material and the auxiliary conductive additives are dissolved together in water, and the negative electrode active material and the auxiliary conductive additives are dissolved together in water.

[0042] The electrode material to be repaired in step (4) is preferably prepared into powder or particles before being added to the repair unit to facilitate sufficient reaction.

[0043] The above-mentioned direct repair of waste battery materials based on redox targeted reactions is applied in the repair of waste lithium-ion battery electrode materials and waste sodium-ion battery electrode materials.

[0044] The present invention adopts energy level matching and ion compensation technology, utilizes the redox reaction between active materials and electrode materials, and directly embeds the missing lithium ions in the waste batteries; it is then integrated with aqueous battery technology into a multifunctional device to achieve the purpose of sustainable compensation of target ions, while promoting the recycling of some reactants in the device.

[0045] The present invention utilizes the different potential energies of the electrochemical reactions occurring at the positive and negative electrodes to form a voltage, so that the ions can be driven by the internal electric field and the selective action of the ion exchange membrane to achieve low-cost and sustainable repair of the positive electrode materials of waste batteries. The repair reaction utilizes the electrolyte that has lost its repair activity due to participating in the peroxidation reaction as a redox medium, and participates in the repair of waste electrode materials in a form similar to a "catalyst". It embeds the missing elements in the waste battery electrode materials back into the lattice through a redox reaction with the waste battery electrode materials, thereby achieving the purpose of directly repairing the electrode materials. It is only necessary to continuously replace the waste battery electrode materials so that the repair active substances are always in a regenerated state, and then the repair reaction can be carried out all the time. It is also effective to add waste battery electrode materials midway.

[0046] The mechanism of the present invention is:

[0047] In aqueous batteries, the cheap metal B (such as Zn, Fe, etc.) at the negative electrode undergoes a reaction at the negative electrode: B (s) -ne - =B n+ At the same time, an oxidation reaction occurs at the positive electrode: A n+ +ne - =A, where A is the reduced state of the above-mentioned positive electrode active material, which is converted into the corresponding oxidized state A after losing electrons n+ . Due to the different potentials of the electrochemical reactions at the positive and negative electrodes, a potential difference is generated. Driven by the potential difference between the positive and negative electrodes and the selective permeability of the ion exchange membrane, the lithium supply solution (or sodium supply solution) in the middle of the energy storage unit will continuously provide lithium ions (or sodium ions) to the repair unit. n+ Coexistence, when driven by the circulation pump into the repair unit, A and O react spontaneously: A+Li + +O=A n+ +R or A+Na + +O=A n+ +R; where O is the positive electrode material of the waste battery to be repaired, and R is the corresponding repaired positive electrode material. This allows the missing ions in the positive electrode material O of the waste battery to be repaired to be embedded back, and at the same time, the positive electrode active material A obtains electrons provided by the cheap metal B of the negative electrode, and regains the repair activity. Since the negative electrode is a cheap metal, combined with the recycling of the positive electrode active material, it can promote the continuous operation of the repair unit, thereby realizing low-cost battery electrode material repair.

[0048] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0049] The present invention uses a targeted redox method to embed lost elements in battery electrode materials in a targeted manner, with a high degree of repair and other uses. The raw materials used are easily available, have low usage requirements, are low in cost, and are environmentally friendly. During the repair process, greenhouse gas emissions and secondary pollution are greatly reduced, further reducing environmental pollution caused by batteries, and have the advantage of sustainable utilization;

[0050] The operation process of the electrochemical continuous repair of electrode materials in the present invention is simple and convenient, and has practical application value in the repair of waste batteries. The method is suitable for large-scale production in factories and can be applied in the treatment of industrial waste, the repair of waste batteries, energy conversion and storage, and other fields that require the use of electrical energy. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 It is a schematic diagram of the electrode material of the repair battery and the three-channel device of aqueous zinc energy storage in the present invention;

[0052] Figure 2 It is a schematic diagram of five acrylic plates in the three-channel device for repairing battery electrode materials and aqueous iron energy storage in the present invention;

[0053] Figure 3 It is the CV curve diagram of ascorbic acid and LiFePO4;

[0054] Figure 4 This is a curve diagram of voltage-discharge time variation of the device in Example 1 when no LiFePO4 is added, that is, ascorbic acid: waste LiFePO4=1:0 (molar ratio);

[0055] Figure 5 The voltage-discharge time variation curve of the device in Example 1 when the amount of LiFePO4 input is ascorbic acid: waste LiFePO4=1:0.5 (molar ratio);

[0056] Figure 6 In Example 1, Figure 5 The change curve of lithium content in the reaction of waste LiFePO4 with 0.1M Vc concentration for different reaction times under different conditions;

[0057] Figure 7 The voltage-discharge time variation curve of the device in Example 1 when the amount of LiFePO4 input is ascorbic acid: waste LiFePO4=1:1 (molar ratio);

[0058] Figure 8 In Example 1, Figure 7 CV curves of button cells and waste LIBs corresponding to LiFePO4 repaired under the same conditions;

[0059] Fig. 9 The XRD patterns of LiFePO4 powder at different reaction times in Example 1;

[0060] Fig.10 The ICP histograms of different repair durations in Example 2;

[0061] Fig.11 This is the SEM image of the NaFePO4 powder after repair for 2 hours in Example 3;

[0062] Fig.12 This is the lattice change during the repair process of waste LiFePO4 in Example 4. DETAILED DESCRIPTION

[0063] The present invention is further described in detail below in conjunction with the examples and drawings, but the embodiments of the present invention are not limited thereto. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0064] Example 1

[0065] A method and application of direct repair of waste battery materials based on redox targeted reaction, wherein the device for continuous repair of LiFePO4 comprises the following operations:

[0066] (I) Preparation of positive and negative electrode current collectors:

[0067] 1) Use scissors to cut out a circular hydrophobic carbon cloth with a diameter of 3.5 cm as the positive electrode;

[0068] 2) Use scissors to cut out a circular ordinary zinc sheet with a diameter of 3.5 cm as the negative electrode;

[0069] (II) Preparation of electrolyte:

[0070] 3) Weigh 0.8592g of potassium dihydrogen phosphate, 16.5035g of potassium dihydrogen phosphate (potassium dihydrogen phosphate and potassium dihydrogen phosphate are used as pH buffer to stabilize the pH of the positive electrode electrolyte at about 4-5), 1.7612g of ascorbic acid, and 5.4972g of Li2SO4 and dissolve them in 100mL of deionized water; after stirring for 4h, a mixed solution of 0.1M ascorbic acid with a pH stable between 4-5 is obtained, which is used as the positive electrode electrolyte;

[0071] 4) Take 25 ml of positive electrolyte as the flowing liquid in chamber I;

[0072] 5) Prepare 100 mL of 1 M zinc salt solution with 99% purity ZnSO4;

[0073] 6) Take 25 ml of the ZnSO4 solution prepared in step 5) and circulate it in chamber III to form a negative electrode electrolyte;

[0074] (III) Preparation of Li2SO4 solution:

[0075] 7) Dissolve anhydrous Li2SO4 in 100 mL of dilute sulfuric acid solution (pH 4) to prepare a Li2SO4 solution with a lithium ion concentration of 1 M;

[0076] 8) Take 15 ml of the Li2SO4 solution prepared in step 7) as the lithium supply solution flowing in chamber II;

[0077] (IV) Device preparation:

[0078] 9) The circular zinc sheet obtained in (I) is used as the negative electrode material, and the circular hydrophobic carbon cloth is used as the positive electrode material; the positive electrode electrolyte obtained in step 4), the negative electrode electrolyte obtained in step 6), the lithium supply solution in step 7), an anion exchange membrane (diameter 4 cm), a cation exchange membrane (diameter 4 cm), 5 acrylic plates (10 cm×10 cm×1 cm), as follows Figure 2 As shown, three of the acrylic plates have cavities (3.5 cm in diameter) to serve as chambers for the circulation of three solutions, and the other two acrylic plates have no cavities and are used to support and seal the device. Figure 1 The schematic structure is assembled into a three-channel aqueous battery device; the device is fixed with studs and nuts, and chambers I, II and III are circulated using a small peristaltic pump respectively;

[0079] 10) A 50 ml cylindrical container is used as the liquid storage tank of the repair unit and is separated into two parts by a glass fiber diaphragm. 1-x FePO4 molar ratio of the repaired LiFePO4 powder (Li 1-x FePO4) is placed in the lower layer so that the LiFePO4 to be repaired can react with the pumped electrolyte, but after being filtered, it will not flow back to the energy storage unit with the solution.

[0080] The redox reaction formula of each part in Example 1 is:

[0081] Repair process x / 2C6H8O6 + xLi + + Li 1-x FePO4 = x / 2C6H6O6 + xH + + LiFePO4

[0082] Battery Process Positive Electrode: C6H6O6 + 2e - + 2H + = C6H8O6

[0083] Anode: Zn-2e - =Zn 2+

[0084] Take 25mL of positive electrolyte and conduct CV test of ascorbic acid in a three-electrode system, where the glassy carbon electrode is the working electrode, the calomel electrode is the reference electrode, and the platinum mesh electrode is the counter electrode; take 25mL of lithium supply solution and conduct CV test of LiFePO4 in a three-electrode system, where LiFePO4 is the working electrode, the calomel electrode is the reference electrode, and the platinum mesh electrode is the counter electrode. The CV curves of ascorbic acid and LiFePO4 are finally obtained as shown in the figure below. Figure 3As shown in the figure, it can be seen that the oxidation peak potential of LiFePO4 is significantly higher than that of ascorbic acid, indicating that LiFePO4 can easily obtain electrons from ascorbic acid and be reduced.

[0085] Figure 4 Ascorbic acid: Li 1-x When FePO4=1:0 (molar ratio), the voltage variation trend and discharge duration of the device self-discharge;

[0086] Figure 5 Ascorbic acid: Li 1-x Device voltage change trend and discharge duration when FePO4=1:0.5 (molar ratio); Figure 6 This is a graph showing the change in lithium content when waste LiFePO4 reacts with 0.1M ascorbic acid concentration for different reaction times.

[0087] Figure 7 Ascorbic acid: Li 1-x When FePO4=1:1 (molar ratio), the voltage variation trend and discharge duration of the device;

[0088] The electrochemical properties of the positive electrode material were tested using a CR2032 button cell. The positive electrode of the battery was an aluminum foil coated with a prepared slurry, which was dispersed in N-methyl-2-pyrrolidone (NMP) with an active material (to be tested LiFePO4), polyvinylidene fluoride (PVDF) and carbon black (Super P) in a mass ratio of 8:1:1 and obtained after vacuum drying at 120°C for 12 hours. A half-cell was assembled in an argon-filled glove box using lithium foil as the negative electrode and Celgard PP2400 membrane as the separator. The electrolyte was a solution of 1M LiPF6 dissolved in EC / DEC / EMC (v / v / v, 1 / 1 / 1). Figure 8 In Example 1, Figure 7 CV curves of button cells and waste LIBs corresponding to LiFePO4 repaired for 2h under the same conditions. After 120min of repair, the performance of the repaired LIBs has significantly exceeded that of the waste LIBs.

[0089] Fig. 9 Li before and after the reaction 1-x FePO4 powder XRD pattern (ascorbic acid: Li 1-x FePO4 = 1:0.5 (molar ratio). After the reaction, the main peak is closer to pure LiFePO4, indicating that the lithium element has been embedded.

[0090] Based on the above data, as the amount of LiFePO4 to be repaired increases, the duration of the lithium insertion reaction of the device can be extended, and the lithium element in the waste LiFePO4 is inserted and repaired under the "catalysis" of the ascorbic acid solution. At the same time, adding waste LiFePO4 in the middle of the reaction has the same effect. Therefore, as long as the LiFePO4 to be repaired that reacts with the redox electrolyte is continuously updated, the repair reaction can be promoted to continue, and the missing lithium element in the electrode material can be continuously inserted back with the help of ascorbic acid.

[0091] Example 2

[0092] A method and application of direct repair of waste battery materials based on redox targeted reaction, wherein the device for continuous repair of LiFePO4 comprises the following operations:

[0093] (I) Preparation of positive and negative electrode current collectors:

[0094] 1) Use scissors to cut out a circular hydrophobic carbon cloth with a diameter of 3.5 cm as the positive electrode;

[0095] 2) Use scissors to cut out a circular iron sheet with a diameter of 3.5 cm as the negative electrode;

[0096] (II) Preparation of electrolyte:

[0097] 3) Weigh 0.8592g of potassium dihydrogen phosphate, 16.5035g of potassium dihydrogen phosphate (potassium dihydrogen phosphate and potassium dihydrogen phosphate are used as pH buffer to stabilize the pH of the positive electrode electrolyte at about 4-5), 1.7612g of ascorbic acid, and 5.4972g of Li2SO4 and dissolve them in 100mL of deionized water; after stirring for 4h, a mixed solution of 0.1M ascorbic acid with a pH stable between 4-5 is obtained, which is used as the positive electrode electrolyte;

[0098] 4) Take 25 ml of positive electrolyte as the flowing liquid in chamber I;

[0099] 5) Prepare 100 mL of 1 M iron salt solution with 99% purity FeSO4;

[0100] 6) Take 25 ml of the FeSO4 solution prepared in step 5) and circulate it in chamber III to form a negative electrode electrolyte;

[0101] (III) Preparation of Li2SO4 solution:

[0102] 7) Dissolve anhydrous Li2SO4 in 100 mL of dilute sulfuric acid solution (pH 4) to prepare a Li2SO4 solution with a lithium ion concentration of 1 M;

[0103] 8) Take 15 ml of the Li2SO4 solution prepared in step 7) as the lithium supply solution flowing in chamber II;

[0104] (IV) Device preparation:

[0105] 9) The circular iron sheet obtained in (I) is used as the negative electrode material, and the circular hydrophobic carbon cloth is used as the positive electrode material; the positive electrode electrolyte obtained in step 4), the negative electrode electrolyte obtained in step 6), the lithium supply solution in step 7), an anion exchange membrane (diameter 4 cm), a cation exchange membrane (diameter 4 cm), 5 acrylic plates (10 cm × 10 cm × 1 cm), 3 of which have cavities (diameter 3.5 cm) for reference Figure 1 The schematic structure is assembled into a three-channel aqueous battery device; the device is fixed with studs and nuts, and chambers I, II and III are circulated using a small peristaltic pump respectively;

[0106] 10) A 50 ml cylindrical container is used as the liquid storage tank of the repair unit and is separated into two parts by a glass fiber diaphragm. 1-x FePO4) is placed in the lower layer, so that the LiFePO4 (Li 1-x FePO4) can react with the pumped electrolyte, but after being filtered, it will not flow back into the energy storage unit with the solution. Ascorbic acid and the LiFePO4 powder to be repaired (Li 1-x The molar ratio of FePO4 is 1:0.5.

[0107] The redox reaction formula of each part in Example 2 is:

[0108] Repair process x / 2C6H8O6+xLi + +Li 1-x FePO4=x / 2C6H6O6+xH + +LiFePO4

[0109] Battery process positive electrode: C6H6O6+2e - +2H + =C6H8O6

[0110] Negative electrode: Fe-2e - =Fe 2+

[0111] Fig.10 This is the ICP bar chart of different repair times when the ascorbic acid concentration is 1M; it can be seen that the Li content continues to increase with the increase of repair time, indicating that this method can increase the lithium content of waste LiFePO4.

[0112] Example 3

[0113] A method and application of direct repair of waste battery materials based on redox targeted reaction, wherein the device for continuous repair of NaFePO4 comprises the following operations:

[0114] (I) Preparation of positive and negative electrode current collectors:

[0115] 1) Use scissors to cut out a circular hydrophobic carbon cloth with a diameter of 3.5 cm as the positive electrode;

[0116] 2) Use scissors to cut out a circular ordinary zinc sheet with a diameter of 3.5 cm as the negative electrode;

[0117] (II) Preparation of electrolyte:

[0118] 3) Weigh 0.4052g of potassium dihydrogen phosphate, 16.5035g of potassium dihydrogen phosphate (potassium dihydrogen phosphate and potassium dihydrogen phosphate are used as pH buffer to stabilize the pH of the positive electrode electrolyte at about 4-5), 1.9811g of sodium ascorbate, and 5.8442g of NaCl and dissolve them in 100mL of deionized water; after stirring for 4h, a mixed solution of 0.1M sodium ascorbate with a pH stable between 4-5 is obtained, which is used as the positive electrode electrolyte;

[0119] 4) Take 25 ml of positive electrolyte as the flowing liquid in chamber I;

[0120] 5) Prepare 100 mL of 1 M zinc salt solution with 99% purity ZnCl2;

[0121] 6) Take 25 ml of the ZnCl2 solution prepared in step 5 and circulate it in chamber III to form the negative electrode electrolyte;

[0122] (III) Preparation of sodium solution NaCl solution:

[0123] 7) Dissolve anhydrous NaCl in 100 mL of dilute hydrochloric acid solution (pH 4) to prepare a 1 M NaCl solution;

[0124] 8) Take 15 ml of the NaCl solution prepared in step 7) as the sodium supply solution flowing in chamber II;

[0125] (IV) Device preparation:

[0126] 9) The circular zinc sheet obtained in (I) is used as the negative electrode material, and the circular hydrophobic carbon cloth is used as the positive electrode material; the positive electrode electrolyte obtained in step 4), the negative electrode electrolyte obtained in step 6), the sodium supply solution in step 7), an anion exchange membrane (diameter 4 cm), a cation exchange membrane (diameter 4 cm), 5 acrylic plates (10 cm × 10 cm × 1 cm), 3 of which have cavities (diameter 3.5 cm), reference Figure 1The schematic structure is assembled into a three-channel aqueous battery device; the device is fixed with studs and nuts, and chambers I, II and III are circulated using a small peristaltic pump respectively;

[0127] 10) A 50 ml cylindrical container is used as the liquid storage tank of the repair unit and is separated into two parts by a glass fiber diaphragm. 1-x FePO4) is placed in the lower layer, so that the NaFePO4 to be repaired can react with the pumped electrolyte, but after being filtered, it will not flow back to the energy storage unit with the solution. Sodium ascorbate (C6H7O6Na) and the NaFePO4 powder to be repaired (Na 1-x The molar ratio of FePO4 is 1:0.5.

[0128] The redox reaction formula of each part in Example 3 is:

[0129] Repair process xC6H7O6Na+Na 1-x FePO4=xC6H6O6+xH + +NaFePO4

[0130] Battery process positive electrode: C6H6O6+2e - +2H + =C6H8O6

[0131] Anode: Zn-2e - =Zn 2+

[0132] Fig.11 This is a SEM image of the NaFePO4 powder to be repaired after 2 hours of repair in Example 3. It can be seen that the particles are evenly distributed, which is beneficial to the migration of sodium ions to a certain extent, suggesting better electrode performance.

[0133] Example 4

[0134] A method and application of direct repair of waste battery materials based on redox targeted reaction, wherein the device for continuous repair of LiFePO4 comprises the following operations:

[0135] (I) Preparation of positive and negative electrode current collectors:

[0136] 1) Use scissors to cut out a circular hydrophobic carbon cloth with a diameter of 3.5 cm as the positive electrode;

[0137] 2) Use scissors to cut out a circular ordinary zinc sheet with a diameter of 3.5 cm as the negative electrode;

[0138] (II) Preparation of electrolyte:

[0139] 3) Weigh 0.8592g of potassium dihydrogen phosphate, 16.5035g of potassium dihydrogen phosphate (to stabilize pH), 1.9212g of citric acid, and 5.4972g of Li2SO4 and dissolve them in 100mL of deionized water; after stirring for 4h, a mixed solution of 0.1M citric acid with a pH stable between 4-5 is obtained, which is used as the positive electrode electrolyte;

[0140] 4) Take 25 ml of positive electrolyte as the flowing liquid in chamber I;

[0141] 5) Prepare 100 mL of 1 M zinc salt solution with 99% purity ZnSO4;

[0142] 6) Take 25 ml of the ZnSO4 solution prepared in step 5 and circulate it in chamber III to form the negative electrode electrolyte;

[0143] (III) Preparation of Li2SO4 solution:

[0144] 7) Dissolve anhydrous Li2SO4 in 100 mL of deionized water to prepare a Li2SO4 solution with a lithium ion concentration of 1 M;

[0145] 8) Take 15 ml of the Li2SO4 solution prepared in step 7) as the lithium supply solution flowing in chamber II;

[0146] (IV) Device preparation:

[0147] 9) The circular zinc sheet obtained in (I) is used as the negative electrode material, and the circular hydrophobic carbon cloth is used as the positive electrode material; the positive electrode electrolyte obtained in step 4), the negative electrode electrolyte obtained in step 6), the lithium supply solution in step 7), an anion exchange membrane (diameter 4 cm), a cation exchange membrane (diameter 4 cm), 5 acrylic plates (10 cm × 10 cm × 1 cm), 3 of which have cavities (diameter 3.5 cm), reference Figure 1 The schematic structure is assembled into a three-channel aqueous battery device; the device is fixed with studs and nuts, and chambers I, II and III are circulated using a small peristaltic pump respectively;

[0148] 10) A 50 ml cylindrical container is used as the liquid storage tank of the repair unit and is separated into two parts by a glass fiber diaphragm. 1-x FePO4) is placed in the lower layer, so that the LiFePO4 to be repaired can react with the pumped electrolyte, but after being filtered, it will not flow back to the energy storage unit with the solution; citric acid (C6H8O7) and the LiFePO4 powder to be repaired (Li 1- x The molar ratio of FePO4 is 0.5.

[0149] The redox reaction formula of each part in Example 4 is:

[0150] Repair process

[0151] x / 2C6H8O7+xLi + +Li 1-x FePO4=x / 2C5H6O5+xH + +x / 2CO2+LiFePO4

[0152] Battery process positive electrode: C5H6O5+2e - +2H + +CO2=C6H8O7

[0153] Anode: Zn-2e - =Zn 2+

[0154] After the device in Example 4 was assembled, an electrode repair test was performed. The lattice structure of the product was tested by XRD, and the unit cell parameters of the repaired product were obtained after refinement. The results are as follows: Fig.12 As shown. It can be seen that with the continuous insertion of lithium ions, Li x The a-axis of the FePO4 unit cell is increasing, suggesting that the lithium ion transmission channel is gradually expanding.

[0155] Example 5

[0156] A method and application of direct repair of waste battery materials based on redox targeted reaction, wherein the device for continuous repair of LiCoO2 comprises the following operations:

[0157] (I) Preparation of positive and negative electrode current collectors:

[0158] 1) Use scissors to cut out a circular hydrophobic carbon cloth with a diameter of 3.5 cm as the positive electrode;

[0159] 2) Use scissors to cut out a circular ordinary zinc sheet with a diameter of 3.5 cm as the negative electrode;

[0160] (II) Preparation of electrolyte:

[0161] 3) Weigh 1.3385g LiI and 5.4972g Li2SO4 and dissolve them in 100mL deionized water; after stirring for 4h, a 0.1M LiI mixed solution is obtained, which is used as the positive electrode electrolyte;

[0162] 4) Take 25 ml of positive electrolyte as the flowing liquid in chamber I;

[0163] 5) Prepare 100 mL of 1 M zinc salt solution with 99% purity ZnSO4;

[0164] 6) Take 25 ml of the ZnSO4 solution prepared in step 5) and circulate it in chamber III to form a negative electrode electrolyte;

[0165] (III) Preparation of Li2SO4 solution:

[0166] 7) Dissolve anhydrous Li2SO4 in 100 mL of deionized water to prepare a Li2SO4 solution with a lithium ion concentration of 1 M;

[0167] 8) Take 15 ml of the Li2SO4 solution prepared in step 7) as the lithium supply solution flowing in chamber II;

[0168] (IV) Device preparation:

[0169] 9) The circular zinc sheet obtained in (I) is used as the negative electrode material, and the circular hydrophobic carbon cloth is used as the positive electrode material; the positive electrolyte obtained in step 4), the negative electrolyte obtained in step 6), the lithium supply solution in step 7), an anion exchange membrane (diameter 4 cm), a cation exchange membrane (diameter 4 cm), 5 acrylic plates (10 cm × 10 cm × 1 cm), 3 of which have cavities (diameter 3.5 cm). Reference Figure 1 The schematic structure is assembled into a three-channel aqueous battery device; the device is fixed with studs and nuts, and chambers I, II and III are circulated using a small peristaltic pump respectively;

[0170] 10) A 50 ml cylindrical container is used as the liquid storage tank of the repair unit and is separated into two parts by a glass fiber diaphragm. 1-x CoO2) is placed in the lower layer, so that the LiCoO2 powder to be repaired can react with the pumped electrolyte, but after being filtered, it will not flow back to the energy storage unit with the solution; LiI and the LiCoO2 powder to be repaired (Li 1-x The molar ratio of CoO2 is 1:0.5.

[0171] The redox reaction formula of each part in Example 5 is:

[0172] Restoration Process 3xI - +2xLi + +2Li 1-x CoO2=xI2+2LiCoO2

[0173] Battery process positive electrode: I2+2e - =3I -

[0174] Anode: Zn-2e - =Zn 2+

[0175] After the device in Example 5 was assembled, the electrochemical performance test was carried out. The ion content of the repaired electrode was tested by ICP to obtain the repair effect of the waste electrode. The results are shown in Table 1 below:

[0176] Table 1 Electrical effects of different lengths of repair of waste LiCoO2 electrodes in Example 5

[0177]

[0178] The above data show that the lithium content in the repaired electrode increases, and the lithium content increases with time until it reaches a peak around 2 hours. This indicates that the solution in the repair chamber accepts Li from the lithium supply solution in chamber II. + and chamber III solution I - The electrons provided enable the waste electrode materials to be reduced and accept the lithium elements enriched in the solution, thereby embedding the missing lithium elements in the waste LiCoO2 batteries and achieving the effect of electrode repair.

[0179] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A direct repair system for waste battery materials based on redox targeted reaction, characterized in that It includes a repair unit and an energy storage unit, wherein: The repair unit is a liquid storage tank containing the battery electrode material to be repaired and a filter membrane; the filter membrane separates the liquid storage tank into two layers, and the battery electrode material to be repaired is placed in the lower layer; the filter membrane allows liquid to pass through, but will intercept solid particles, realizing solid-liquid separation in the repair unit; The energy storage unit is constructed based on an aqueous battery, which includes a positive electrode current collector, a positive electrode electrolyte, a lithium supply solution or a sodium supply solution, a negative electrode electrolyte and a negative electrode current collector in sequence. Different solutions are divided into different chambers by ion exchange membranes to achieve different functions; the solutions in each chamber are circulated by a circulating pump; The repair unit is connected to the positive electrode electrolyte of the energy storage unit through a circulation pump and a pipeline to form a circulation, that is, the positive electrode electrolyte is pumped out from the energy storage unit, enters the lower layer of the repair unit, directly contacts and reacts with the battery electrode material to be repaired, and then is filtered through a filter membrane to achieve solid-liquid separation from the battery electrode material to be repaired, enters the upper layer of the repair unit, and finally flows back to the positive electrode electrolyte of the energy storage unit.

2. The direct repair system for waste battery materials based on redox targeted reaction according to claim 1 is characterized in that: The battery electrode material to be repaired is a lithium battery electrode material or a sodium battery electrode material, preferably at least one of LiFePO4, LiNiO2, LiCoO2, Na3MnTi(PO4)3, Na3V2(PO4)3, ternary NCA or NCM electrode materials.

3. The direct repair system for waste battery materials based on redox targeted reaction according to claim 1 is characterized in that: The filter membrane is at least one of a glass fiber membrane, filter paper, nylon filter membrane, polytetrafluoroethylene filter membrane, mixed cellulose filter membrane, polyethersulfone filter membrane, polypropylene filter membrane and polyvinylidene fluoride filter membrane; the interception particle size of the filter membrane is 0.1 to 50 μm; The ion exchange membrane includes at least one of an anion exchange membrane and a cation exchange membrane.

4. The direct repair system for waste battery materials based on redox targeted reaction according to claim 1 is characterized in that: The positive electrode current collector is a conductive carrier; wherein the conductive carrier comprises at least one of carbon cloth, hydrophobic carbon cloth, carbon paper, graphite paper, zinc sheet, aluminum foil, copper foil, and foam metal; The negative electrode current collector is a negative electrode active material or a conductive carrier; the negative electrode active material includes one of Cu, Sn, Pb, Zn, Fe, Ga, and Mn electrode materials; the conductive carrier includes at least one of carbon cloth, hydrophobic carbon cloth, carbon paper, graphite paper, zinc sheet, aluminum foil, copper foil, and foam metal; The positive electrode electrolyte is an aqueous solution containing positive electrode active materials, wherein the positive electrode active materials are materials with redox activity, including but not limited to ascorbic acid, citric acid, magnesium ascorbate, sodium ascorbate, [Fe(CN)6] 3- , [Fe(CN)6] 4- 、FeCl2、TEMPO、I - , BTMAP-Fc, FcNCl or FcN2Br2; the concentration of the positive electrode active substance in the positive electrode electrolyte is ≥10mM, and the pH range should be between 2-7; When the negative electrode current collector is a negative electrode active material, the negative electrode electrolyte is water or an aqueous solution containing a salt of the corresponding negative electrode active material, and the concentration of the salt of the corresponding negative electrode active material is ≥10mM; when the negative electrode current collector is a conductive carrier, the negative electrode electrolyte is an aqueous solution of a negative electrode active material, wherein the negative electrode active material is V 2+ Cr 2+ 、Ti 3+ and one of I2.

5. The direct repair system for waste battery materials based on redox targeted reaction according to claim 4 is characterized in that: The positive electrode electrolyte also includes an auxiliary conductive additive, the type of which is determined by the goal of the direct repair system and maintains anion consistency with the lithium supply solution or sodium supply solution in the adjacent chamber; The negative electrode electrolyte also includes an auxiliary conductive additive, the type of which is determined by the goal of the direct repair system, and maintains cation consistency with the negative electrode active material; and maintains anion consistency with the lithium supply solution or sodium supply solution in the adjacent chamber.

6. The direct repair system for waste battery materials based on redox targeted reaction according to claim 5 is characterized in that: The auxiliary conductive additives in the positive and negative electrode electrolytes relatively independently include at least one of NaCl, NaF, Na2SO4, KCl, LiCl, LiF, Li2SO4, ZnSO4, ZnCl2, FeSO4 and FeCl2, CH3COOLi2 and LiNO3; the concentrations of the auxiliary conductive agents in the positive electrode electrolyte and the negative electrode electrolyte are relatively independently 0M to 1M.

7. The direct repair system for waste battery materials based on redox targeted reaction according to claim 1 is characterized in that: The lithium supply solution is a solution containing lithium metal ions, preferably at least one of Li2SO4 solution, LiCl solution, LiF solution, LiNO3 solution, and CH3COOLi2 solution; the concentration of the lithium supply solution is relatively independent and is 0.1M to 3M; The sodium supply solution is a solution containing sodium metal ions, preferably at least one of NaCl solution, Na2SO4 solution, NaNO3 solution, NaF solution, and CH3COONa2 solution; the concentration of the sodium supply solution is relatively independent and is 0.1M to 3M.

8. A method for directly repairing waste battery materials based on redox targeted reaction, characterized in that The following steps are involved: (1) Preparing a positive electrode electrolyte, a negative electrode electrolyte, and a lithium supply solution or a sodium supply solution: uniformly dissolving a positive electrode active material, a negative electrode active material, and a lithium supply material or a sodium supply material in water to obtain a positive electrode electrolyte, a negative electrode electrolyte, and a lithium supply solution or a sodium supply solution; (2) assembling a lithium supply solution or a sodium supply solution, a positive electrode electrolyte, a negative electrode electrolyte, a positive electrode current collector material, a negative electrode current collector material, and an ion exchange membrane into an aqueous battery device, i.e., an energy storage unit; (3) The positive electrode electrolyte in the energy storage unit is pumped out, and after direct contact and reaction with the electrode material to be repaired in the repair unit, the solution and the electrode material to be repaired are separated by a filtration membrane and flowed back to the energy storage unit to promote the continuation of the repair reaction; the reaction of the repair process is: A+Li + +O=A n+ +R or A+Na + +O=A n+ +R; O is the cathode material to be repaired, and R is the cathode material after repair; O is reduced by A and its valence state is reduced, and then Li in the lithium supply solution is obtained. + To achieve charge balance, thereby replenishing the missing Li; or to obtain Na in the sodium supply solution + , replenish the missing Na and complete the repair process; (4) When the positive electrode electrolyte flows back from the repair unit, the energy storage unit circuit is closed. Due to the different potentials of the redox reactions at both ends, a potential difference is generated, which supplies power to the reduction active material and drives the repair reaction to proceed continuously. The reaction at the positive electrode is: A n+ +ne - =A; the reaction at the negative electrode is: B-ne - =B n+ ; Wherein A is the reduced state of the above-mentioned positive electrode active material, A n+ is the corresponding oxidation state; and B corresponds to the reduced state of the above-mentioned negative electrode active material, B n+ is the corresponding oxidation state.

9. The method for direct repair of waste battery materials based on redox targeted reaction according to claim 8, characterized in that: When the positive electrode electrolyte and the negative electrode electrolyte described in step (1) further include an auxiliary conductive additive, the positive electrode active material and the auxiliary conductive additive are dissolved together in water, and the negative electrode active material and the auxiliary conductive additive are dissolved together in water; In step (4), the electrode material to be repaired is first prepared into powder or particles before being added to the repair unit to facilitate sufficient reaction.

10. Use of the direct repair system for waste battery materials based on redox targeted reaction according to any one of claims 1 to 7 in repairing waste lithium-ion battery electrode materials and waste sodium-ion battery electrode materials.

Citation Information

Patent Citations

  • Recycling and regeneration of lithium ion battery cathodes

    CN116457981A

  • Targeted redox-driven electrochemical desalination, ion extraction and electrode material recovery method and application

    CN116706301A

  • Design method for realizing high-capacity seawater relay desalination and large-scale energy storage by using serial oxidation reduction

    CN117105353A

  • Waste lithium iron phosphate recycling and regenerating method based on redox targeted flow battery

    CN117393874A