Styrene resin molded article
By using a gauge polystyrene resin and low dielectric glass in a styrene resin molded body, the dielectric constant and crystallization temperature are controlled, and the balance between heat resistance and dielectricity is solved, and the low dielectricity is achieved The combination of electrical properties and high heat resistance is suitable for high-frequency electronic devices.
Patent Information
- Application Number
- CN202380029236.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-25
- Filing Date
- 2023-03-09
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, when improving the heat resistance of circuit substrates, it is often necessary to increase the amount of inorganic compounds, resulting in an increase in dielectric constant and an increase in transmission loss, making it difficult to find a balance between low dielectricity and high heat resistance.
采用含有间规聚苯乙烯系树脂的苯乙烯系树脂成形体,通过添加低介电玻璃作为低介电填料,并在不增加传输损耗的前提下提升耐热性,介电常数控制在10GHz频率下的5.5F/m以下,升温结晶温度设为180℃以下,降温结晶温度设为260℃以下,结晶度为30%以上,线膨胀系数为200ppm以下。
It is realized that the heat resistance and low dielectricity of the styrene-based resin molded body are improved without increasing transmission loss, and is suitable for electronic equipment and communication equipment in high-frequency band areas.
Smart Images

Figure BDA0005052683310000181 
Figure BDA0005052683310000191
Abstract
Description
Technical Field
[0001] The present invention relates to a styrene resin molded body containing a syndiotactic polystyrene resin and a substrate which is a laminate of the styrene resin molded body and a metal film. Background Art
[0002] In recent years, in order to increase the speed of information processing in the fields of personal computers (PCs) and mobile phones, frequencies in the high-frequency band region of more than 1 GHz have been adopted. Therefore, for circuit substrates and other electronic components assembled in personal computers, mobile phones, etc., lower transmission losses in the high-frequency band region are sought. Transmission loss refers to the degree of degradation of electrical signals and optical signals circulating on communication lines. Transmission loss is consumed as heat energy and released as heat, so it is not preferred.
[0003] For reducing transmission loss, it is possible to consider using low dielectric polymer materials with low dielectric loss. As low dielectric polymer materials, for example, known: thermoplastic resins such as polyolefins and fluorine resins, unsaturated polyester resins, polyimide resins, epoxy resins, vinyl triazine resins (BT resins), cross-linked polyphenylene ethers, thermosetting resins such as curable polyphenylene ethers, etc. (for example, reference to Patent Document 1).
[0004] In addition, since the soldering process is required when assembling the above-mentioned circuit substrates and other electronic components into devices such as personal computers and mobile phones, the above-mentioned low dielectric polymer materials are also required to have heat resistance. As heat resistance, it is required that the material does not deform even when the soldering process is performed, specifically, it is required that the material does not deform even when heated at 260°C for 120 seconds.
[0005] As a method for improving heat resistance, it is known to add inorganic compounds such as glass fibers to polymer materials. However, in order to obtain sufficient heat resistance, a large amount of inorganic compounds need to be added, which leads to problems such as increased dielectric constant of the resin molding and increased transmission loss. That is, the dielectric constant of the inorganic compound is usually as high as 4F / m or more, so the more the amount of inorganic compound added, the higher the dielectric constant of the resin molding as a whole, and the higher the transmission loss.
[0006] Patent Document 2 describes a low dielectric / heat-resistant styrene resin composition having low dielectric properties and high heat resistance. The styrene resin composition contains 1 to 10 parts by weight of an inorganic filler and 1 to 10 parts by weight of an intercalant for the inorganic filler relative to 100 parts by weight of a syndiotactic polystyrene resin. Clay is used as the inorganic filler, and N-phenylmaleimide is used as the intercalant.
[0007] In addition, Patent Document 3 describes a low dielectric / heat-resistant resin composition having low dielectric properties and high heat resistance, which is composed of 100 parts by weight of a syndiotactic polystyrene resin and 1 to 10 parts by weight of an interlayer modified clay obtained by sandwiching distearyl dimethyl ammonium chloride in the interlayer domain. Prior art literature Patent Literature
[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 11-60645 Patent Document 2: Japanese Patent Application Publication No. 2004-323650 Patent Document 3: Japanese Patent Application Publication No. 2005-213317 Summary of the invention Problems to be solved by the invention
[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a styrene resin molded article containing a syndiotactic polystyrene resin, which has low transmission loss and is heat-resistant. Technical means to solve the problem
[0010] The present invention is as follows. [1] A styrene resin molded article, which is a styrene resin molded article containing a syndiotactic polystyrene resin, and contains 1 to 50 parts by mass of a low dielectric filler having a dielectric constant of 5.5 F / m or less at a frequency of 10 GHz, based on 100 parts by mass of the entire resin molded article. [2] The styrene resin molded article according to [1], wherein the low dielectric filler is low dielectric glass. [3] The styrene resin molded article according to [2], wherein the low dielectric glass contains 10 to 30% by mass of B2O3. [4] The styrene resin molded article according to any one of [1] to [3], further comprising 50 parts by mass or less of a high dielectric inorganic filler having a dielectric constant exceeding 5.5 F / m at a frequency of 10 GHz, based on 100 parts by mass of the entire resin molded article. [5] The styrene resin molded article according to any one of [1] to [4], wherein the temperature of the molded article is 180° C. or lower. [6] The styrene resin molded article according to any one of [1] to [5], which has a cooling crystallization temperature of 260°C or less and a crystallinity of 30% or more. [7] The styrene resin molded article according to any one of [1] to [6], which has a linear expansion coefficient of 200 ppm or less. [8] The styrene resin molded article according to any one of [1] to [7], which has an L value of 70 or more and a gloss value of 30% or more. [9] The styrene resin molded article according to any one of [1] to [8], which is used for electronic equipment or communication equipment used in a high frequency band of 1 GHz or more.
[10] The styrene resin molded article according to any one of [1] to [9], which is a film.
[11] A substrate which is a laminate of the styrene resin molded article according to any one of [1] to [9] and a metal film as a film. Effects of the Invention
[0011] According to the present invention, as a styrene resin molded body containing syndiotactic polystyrene resin, it contains a low dielectric filler having a dielectric constant of 5.5 F / m or less at a frequency of 10 GHz. By using syndiotactic polystyrene resin as a base resin, the low dielectric constant and a certain degree of heat resistance of the resin molded body can be ensured, and by making the syndiotactic polystyrene resin contain a low dielectric filler, the heat resistance can be improved without increasing the transmission loss. DETAILED DESCRIPTION
[0012] The styrene resin molded body of the present invention contains a syndiotactic polystyrene resin, and contains 1 to 50 parts by weight of a low dielectric filler having a dielectric constant of 5.5 F / m or less at a frequency of 10 GHz, based on 100 parts by weight of the resin molded body as a whole. According to the styrene resin molded body of the present invention, heat resistance can be improved without increasing transmission loss. This is described in detail below.
[0013] (Syndiotactic polystyrene resin) The resin molding contains a syndiotactic polystyrene resin. A syndiotactic polystyrene resin refers to a resin in which the benzene rings contained in adjacent styrene units are alternately arranged at a high ratio relative to the plane formed by the main chain of the polymer block (hereinafter referred to as syndiotactic tacticity). It means a polystyrene having a syndiotactic tacticity of usually 75 mol% or more, preferably 85 mol% or more, in terms of syndiotactic diads (r); or usually 30 mol% or more, preferably 50 mol% or more, in terms of syndiotactic pentads (rrrr).
[0014] The carbon isotope-based nuclear magnetic resonance method ( 13 C-NMR) to quantitatively identify whether the benzene rings are arranged alternately relative to the plane formed by the main chain of the polymer block. 13The C-NMR method quantitatively measures the existence ratio of each monomer unit using a plurality of consecutive structural units, for example, two consecutive monomer units as a diad, three monomer units as a triad, and five monomer units as a pentad.
[0015] As the syndiotactic polystyrene resin, polystyrene, poly(alkylstyrene), poly(halogenated styrene), poly(halogenated alkylstyrene), poly(alkoxystyrene), poly(vinyl benzoate) and hydrogenated polymers thereof are preferred, and further, a mixture of two or more selected from these, and at least one selected from copolymers containing these as main components. As poly(alkylstyrene), for example, poly(methylstyrene), poly(ethylstyrene), poly(isopropylstyrene), poly(tert-butylstyrene), poly(phenylstyrene), poly(vinylnaphthalene), poly(vinylstyrene) and the like can be mentioned. As poly(halogenated styrene), for example, poly(chlorostyrene), poly(bromostyrene), poly(fluorostyrene) and the like can be mentioned. As poly(halogenated alkylstyrene), for example, poly(chloromethylstyrene) and the like can be mentioned. As poly(alkoxystyrene), for example, poly(methoxystyrene), poly(ethoxystyrene) and the like can be mentioned. Among these, preferred styrene polymers include polystyrene, poly(p-methylstyrene), poly(m-methylstyrene), poly(p- or tert-butylstyrene), poly(p-chlorostyrene), poly(m-chlorostyrene), poly(p-fluorostyrene), hydrogenated polystyrene, and copolymers containing these structural units. In view of the ease of modifying the para position of styrene and the ease of introducing ion exchange groups, a homopolymer of styrene (polystyrene) is particularly preferred. One or more syndiotactic polystyrene resins may be used.
[0016] Taking the resin molding as a whole as 100 parts by mass, the resin molding preferably contains 50 to 90 parts by mass of syndiotactic polystyrene resin. By making the content of syndiotactic polystyrene resin more than 50 parts by mass, the low dielectric constant and heat resistance of the resin molding can be combined. The content of syndiotactic polystyrene resin is more preferably more than 55 parts by mass, and more preferably more than 60 parts by mass. In addition, by setting the content of syndiotactic polystyrene resin to less than 90 parts by mass, the dielectric constant of the resin molding can be suppressed from increasing, and the transmission loss can be suppressed. The content of syndiotactic polystyrene resin is more preferably less than 85 parts by mass, and more preferably less than 80 parts by mass.
[0017] The syndiotactic polystyrene resin can be produced by a known method. As the syndiotactic polystyrene resin, for example, "XAREC" manufactured by Idemitsu Kosan Co., Ltd. can be used.
[0018] (Low dielectric filler) The resin molding contains a low dielectric filler. Relative to the syndiotactic polystyrene resin, by mixing a predetermined amount of low dielectric filler, the heat resistance can be improved without increasing the transmission loss. As a low dielectric filler, it refers to a filler having a dielectric constant of 5.5F / m or less at a frequency of 10GHz. The dielectric constant of the low dielectric filler is preferably less than 5.0F / m, and more preferably less than 4.8F / m. For the dielectric constant of the low dielectric filler, the cavity resonator perturbation method can be used to measure it.
[0019] The low dielectric filler may be an inorganic filler and / or an organic filler, and preferably at least an inorganic filler is used. As the inorganic filler, for example, an inorganic filler containing boron nitride or an inorganic filler containing SiO2 is preferably used.
[0020] When the low dielectric filler is an inorganic filler containing boron nitride, the low dielectric filler as a whole is 100% by mass, preferably containing 80% by mass or more of boron nitride, more preferably containing 90% by mass or more, further preferably containing 95% by mass or more, and most preferably containing 100% by mass. The dielectric constant of boron nitride at a frequency of 10 GHz is 4.5 F / m. As boron nitride, for example, spherical nano-sized "BN" manufactured by Denka can be used.
[0021] When the low dielectric filler is an inorganic filler containing SiO2, based on the low dielectric filler as a whole being 100 mass%, it preferably contains 45 to 99 mass% of SiO2, more preferably 48 mass% or more, further preferably 50 mass% or more, even more preferably 95 mass% or less, and even more preferably 90 mass% or less.
[0022] As the low dielectric filler, for example, low dielectric glass can be used. Low dielectric glass refers to glass having a dielectric constant of 5.5 F / m or less at a frequency of 10 GHz.
[0023] The low dielectric glass preferably contains 45 to 90% by mass of SiO2, taking the entire low dielectric glass as 100% by mass. The content of SiO2 is more preferably 48% by mass or more, further preferably 50% by mass or more, still more preferably 85% by mass or less, and still more preferably 80% by mass or less.
[0024] The low dielectric glass preferably further contains B2O3, and the content of B2O3 is preferably 10 to 30% by mass, based on the entire low dielectric glass being 100% by mass. The transmission loss can be reduced by containing B2O3 in this range. Based on the entire low dielectric glass being 100% by mass, the content of B2O3 is more preferably 12% by mass or more, further preferably 13% by mass or more, still more preferably 28% by mass or less, and still further preferably 25% by mass or less.
[0025] The low dielectric glass preferably further contains CaO, and when the low dielectric glass as a whole is 100% by mass, the content of CaO is preferably 0.01 to 20% by mass. By setting the content of CaO to 0.01% by mass or more, costs can be reduced. The content of CaO is more preferably 0.05% by mass or more, and more preferably 0.1% by mass or more. On the other hand, when the mass of CaO is excessive, the dielectric constant of the resin molding tends to increase. Therefore, the content of CaO is preferably 20% by mass or less. The content of CaO is more preferably 15% by mass or less, and more preferably 13% by mass or less.
[0026] The low dielectric glass may further contain SrO, but when the low dielectric glass as a whole is 100% by mass, the content of SrO is preferably 0.150% by mass or less. By setting the content of SrO to 0.150% by mass or less, the dielectric constant of the resin molded body can be reduced. The content of SrO is more preferably 0.120% by mass or less, and further preferably 0.080% by mass or less. A smaller SrO content is preferred as much as possible, but when it is reduced to less than 0.001% by mass, the productivity will decrease. Therefore, the content of SrO is preferably 0.001% by mass or more.
[0027] As low-dielectric glass, for example, low-dielectric glass "HTD-09100T" manufactured by TOCHU, hollow glass microspheres "Q-CEL (registered trademark) 5020FPS" and "Q-CEL (registered trademark) 7040S" manufactured by Potters-Ballotini, etc. can be used. The shape of the low-dielectric filler is not particularly limited, and it can be a solid structure or a hollow structure, but a hollow structure is preferred. By using a low-dielectric filler with a hollow structure, the dielectric constant of the resin molded body can be reduced. The low-dielectric filler can be surface-treated using a coupling agent. As coupling agents, silane coupling agents, titanate coupling agents, silicone oligomers, etc. can be mentioned.
[0028] As an organic filler, for example, a foaming resin can be used. A foaming resin refers to a resin that is foamed by heating to generate, for example, nitrogen, carbon dioxide, carbon monoxide, ammonia, water vapor, etc. For example, it is preferable to use a resin that is foamed by heating to above 250°C. By containing a small amount of foaming resin, the dielectric constant of the resin molded body can be reduced. As a foaming agent, for example, sodium bicarbonate, ammonium carbonate, etc. can be used. As a resin, for example, an acrylic resin can be used. The foaming resin can be manufactured, for example, by a method of mixing a foaming agent with a thermoplastic resin; or a method of bringing nitrogen and carbon dioxide in a supercritical state into contact with a resin. As an organic filler, for example, the foaming beads "Advancell EM501" manufactured by Sekisui Chemical Co., Ltd. can be used.
[0029] When both an inorganic filler and an organic filler are used as the low dielectric filler, the ratio of the mass of the inorganic filler used as the low dielectric filler to the mass of the organic filler (inorganic filler / organic filler) is, for example, preferably 10 to 20. The ratio of the mass of the inorganic filler to the mass of the organic filler is more preferably 11 or more, further preferably 12 or more, further preferably 19 or less, and further preferably 18 or less.
[0030] Assuming that the resin molding as a whole is 100 parts by mass, the resin molding contains a low dielectric filler in the range of 1 to 50 parts by mass. When the content of the low dielectric filler is less than 1 part by mass, the heat resistance cannot be improved. In addition, it is difficult to control the heating crystallization temperature of the resin molding below a predetermined value. Therefore, the content of the low dielectric filler is more than 1 part by mass, preferably more than 3 parts by mass, and more preferably more than 5 parts by mass. However, when the content of the low dielectric filler exceeds 50 parts by mass, the dielectric constant of the resin molding increases and the transmission loss increases. In addition, the heating crystallization temperature of the resin molding cannot be controlled below a predetermined value. Therefore, the content of the low dielectric filler is less than 50 parts by mass, preferably less than 45 parts by mass, and more preferably less than 40 parts by mass.
[0031] When the resin molded body contains low dielectric glass, the content of the low dielectric glass is preferably 90 mass % or more, more preferably 95 mass % or more, further preferably 98 mass % or more, and most preferably 100 mass % based on 100 mass % of the entire low dielectric filler.
[0032] In the resin molded body, the mass ratio of the low dielectric filler to the syndiotactic polystyrene resin (low dielectric filler / syndiotactic polystyrene resin) preferably satisfies the range of 0.05 to 0.65. The mass ratio of the low dielectric filler to the syndiotactic polystyrene resin is more preferably 0.1 or more, further preferably 0.15 or more, more preferably 0.6 or less, and further preferably 0.55 or less.
[0033] (High dielectric inorganic filler) The resin molded body may also contain a high dielectric inorganic filler having a dielectric constant exceeding 5.5 F / m at a frequency of 10 GHz. The heat resistance may be further improved by containing a high dielectric inorganic filler. The high dielectric inorganic filler preferably has a dielectric constant of 10 F / m or less at a frequency of 10 GHz. The dielectric constant of the high dielectric inorganic filler may be measured by a resonant cavity perturbation method.
[0034] The high dielectric inorganic filler preferably contains SiO2. When the high dielectric inorganic filler contains SiO2, it preferably contains 45 to 90% by mass of SiO2, based on 100% by mass of the entire high dielectric inorganic filler. The content of SiO2 is more preferably 48% by mass or more, further preferably 50% by mass or more, more preferably 85% by mass or less, and further preferably 80% by mass or less.
[0035] The high dielectric inorganic filler may further contain B2O3, but the B2O3 content is preferably less than 10% by mass based on 100% by mass of the high dielectric inorganic filler. The B2O3 content is more preferably less than 9% by mass, and further preferably less than 8% by mass based on 100% by mass of the high dielectric inorganic filler.
[0036] The high dielectric inorganic filler may further contain CaO. When the high dielectric inorganic filler as a whole is 100% by mass, the content of CaO is 15% by mass or more, more preferably more than 20% by mass, and more preferably 21% by mass or more. The upper limit of the content of CaO is, for example, preferably 40% by mass or less, more preferably 35% by mass or less, and more preferably 30% by mass or less.
[0037] The high dielectric inorganic filler may further contain SrO. When the entire high dielectric inorganic filler is 100 mass %, the content of SrO is preferably more than 0.150 mass %, more preferably 0.160 mass % or more, and even more preferably 0.170 mass % or more.
[0038] As the high dielectric inorganic filler, for example, "EPH80M-01N" manufactured by Nippon Electric Glass Co., Ltd. can be used.
[0039] The amount of the high dielectric inorganic filler contained in the resin molded body is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, further preferably 30 parts by mass or less, and even 0 parts by mass is not a problem.
[0040] When the resin molded body contains a high dielectric inorganic filler, the mass ratio of the high dielectric inorganic filler to the low dielectric filler (high dielectric inorganic filler / low dielectric filler) is preferably 0.8 to 1.2. The mixing ratio of the high dielectric inorganic filler to the low dielectric filler is more preferably 0.9 or more, further preferably 0.95 or more, still more preferably 1.1 or less, and still more preferably 1.05 or less.
[0041] (Heating crystallization temperature (hereinafter referred to as Tc1)) The heating crystallization temperature (Tc1) of the resin molding is preferably below 180°C. The heating crystallization temperature (Tc1) refers to the temperature of the most part of the heat peak observed when the temperature is increased. By setting the heating crystallization temperature of the resin molding to below 180°C, the heat resistance (reflow soldering heat resistance) and linear expansion characteristics can be further improved. The heating crystallization temperature of the resin molding is more preferably below 175°C, and further preferably below 170°C. The heating crystallization temperature of the resin molding is preferably as low as possible, but the lower limit is usually around 110°C. The heating crystallization temperature of the resin molding can be measured, analyzed and calculated, for example, by a differential scanning calorimeter (hereinafter referred to as DSC).
[0042] (Crystallization temperature (hereinafter referred to as Tc2)) The cooling crystallization temperature (Tc2) of the resin molded body is preferably below 260°C. The cooling crystallization temperature (Tc2) refers to the temperature of the most part of the heat peak observed during cooling. By setting the cooling crystallization temperature of the resin molded body to below 260°C, productivity can be improved. The cooling crystallization temperature of the resin molded body is more preferably below 255°C, and further preferably below 250°C. The lower limit of the cooling crystallization temperature of the resin molded body is preferably above 180°C. By setting the cooling crystallization temperature of the resin molded body to above 180°C, heat resistance (reflow soldering heat resistance) and linear expansion characteristics can be improved. The cooling crystallization temperature of the resin molded body is more preferably above 190°C, and further preferably above 200°C. The cooling crystallization temperature of the resin molded body can be calculated, for example, by differential scanning calorimetry (DSC) measurement and analysis.
[0043] (Crystallinity) The crystallinity of the resin molding is preferably 30% or more. The crystallinity refers to the value calculated by the ratio of the latent heat of the melting point and the latent heat of the crystallization temperature (Tc2) at the cooling temperature. By setting the crystallinity of the resin molding to 30% or more, the heat resistance (reflow soldering heat resistance) and linear expansion characteristics can be improved. The crystallinity of the resin molding is more preferably 35% or more, and further preferably 40% or more. The crystallinity of the resin molding is preferably as large as possible, even 100%. The crystallinity of the resin molding can be calculated, for example, by differential scanning calorimetry (DSC) measurement and analysis.
[0044] The heating crystallization temperature, cooling crystallization temperature and crystallinity of the resin molded body can be controlled, for example, by adjusting the content of low dielectric filler contained in the resin molded body or adjusting the temperature of the cooling contact roller used in the manufacturing process. Since the resin molded body can be quenched by adjusting the temperature of the cooling contact roller to below 150°C, the heating crystallization temperature of the resin molded body, the cooling crystallization temperature of the resin molded body and the crystallinity can be reduced. Furthermore, since the resin molded body can be prevented from being excessively softened, productivity can be improved. The temperature of the cooling contact roller is preferably below 120°C, and more preferably below 100°C. The lower limit of the temperature of the cooling contact roller is preferably above 10°C. Since the adhesion of water droplets to the cooling contact roller can be prevented by setting the temperature of the cooling contact roller to above 10°C, the appearance of the resin molded body can be made good. The temperature of the cooling contact roller is more preferably above 15°C, and further preferably above 25°C.
[0045] Although the resin molded body thus obtained has sufficient heat resistance as it is, it is also possible to apply heat treatment to the resin molded body. By applying heat treatment, the heat resistance of the resin molded body can be further improved. In addition, by applying heat treatment, the linear expansion coefficient of the resin molded body can be reduced.
[0046] As the conditions for heat treatment, for example, heating is preferably performed within a temperature range of 80°C to 240°C, more preferably above 100°C, further preferably above 150°C, still more preferably below 220°C, and still further preferably below 210°C. By setting the heating temperature to above 80°C, the heat resistance of the resin molded body can be further improved. In addition, the linear expansion coefficient of the resin molded body can be reduced. However, when the heating temperature is too high, there is a possibility that the resin molded body is deformed, so it is preferred to set the heating temperature to below 240°C. There is no particular limitation on the method of applying heat treatment to the resin molded body, and examples thereof include heat setting and electron beam irradiation, preferably heat setting. In the case of heat setting, for example, a method of heat treatment by heating in a dryer can be cited.
[0047] The linear expansion coefficient of the resin molded body is preferably less than 200ppm. Since the linear expansion coefficient of the resin molded body is less than 200ppm, it is difficult to produce deformation caused by heat. The linear expansion coefficient of the resin molded body is more preferably less than 190ppm, and further preferably less than 180ppm. The lower limit of the linear expansion coefficient of the resin molded body is, for example, preferably more than 80ppm, more preferably more than 90ppm, and further preferably more than 100ppm. The linear expansion coefficient of the resin molded body can be measured, for example, using a thermomechanical analysis device. The linear expansion coefficient of the resin molded body can be controlled by adjusting the content of the low dielectric filler contained in the resin molded body and the temperature when applying the heat treatment.
[0048] The resin molded article preferably has a good appearance. Specifically, it is preferred that the L value is 70 or more or the gloss value is 30% or more, and more preferably the L value is 70 or more and the gloss value is 30% or more.
[0049] (L value) The L value (color value L) of the resin molding is preferably 70 or more. The L value is a scale indicating brightness. The larger the value, the less blackening and the higher the brightness, the better the appearance of the resin molding, and the improved product value. The L value of the resin molding is more preferably 73 or more, and further preferably 75 or more. The upper limit of the L value of the resin composition is not particularly limited, and can also be 100, or can be less than 90. When measuring the L value, a colorimeter ("TC-1500MC-88 type" manufactured by Tokyo Denshoku Co., Ltd., etc.) is used, and light source C is used as the standard light, and light is irradiated to the central part of the test piece to obtain the L value of the Lab color system.
[0050] (Gloss value) The gloss value of the resin molded body is preferably 30% or more. By setting the gloss value of the resin molded body to 30% or more, the appearance of the resin molded body is good and the product value is improved. The gloss value of the resin molded body is more preferably 35% or more, and further preferably 40% or more. The upper limit of the gloss value of the resin molded body is not particularly limited, but is, for example, about 90%. The gloss value of the resin molded body can be measured and analyzed by a gloss meter.
[0051] The L value and gloss value of the resin molded body can be controlled by adjusting the content of the low dielectric filler contained in the resin molded body or the surface roughness Rz of the cooling touch roller used in the production. The surface roughness Rz of the cooling touch roller used in the production process is preferably adjusted to 110 μm or less, more preferably 100 μm or less, further preferably 80 μm or less, and particularly preferably 50 μm or less.
[0052] The resin molded body can be suitably used as a material for electronic devices or communication devices used in a high frequency band of 1 GHz or higher, because the transmission loss can be suppressed low even when used in the high frequency band.
[0053] The dielectric constant (εr) of the resin molded body at a frequency of 10 GHz measured by a cavity perturbation method is preferably 3.2 F / m or less. If the dielectric constant at a frequency of 10 GHz is too high, it is difficult to use for applications such as 5G communication equipment and vehicle-mounted radar.
[0054] The dielectric loss tangent (Df) of the resin molded body is preferably 0.002 or less. By setting the dielectric loss tangent of the resin molded body to 0.002 or less, even if an AC electric field is applied, part of its energy can be suppressed from being lost as heat. The dielectric loss tangent (Df) of the resin molded body is more preferably 0.0015 or less, and further preferably 0.0013 or less. The dielectric loss tangent can be measured at a frequency of 10 GHz by a resonant cavity perturbation method.
[0055] The shape of the resin molded body is not particularly limited, and examples thereof include films, sheets, plates, etc., preferably films. The thickness of the film is, for example, preferably 0.1 mm to 1 mm, more preferably 0.15 mm or more, further preferably 0.2 mm or more, still more preferably 0.9 mm or less, and further preferably 0.8 mm or less.
[0056] The present invention also includes a substrate which is a laminate of the resin molded body film and the metal film according to the present invention. The substrate can be suitably used as a material for electronic devices or communication devices used in a high frequency band region of 1 GHz or more.
[0057] Examples of the metal film include films of copper, aluminum, iron, stainless steel, nickel, and alloy films thereof, and a copper film is most preferred among these.
[0058] The styrene resin molded article of the present invention can be produced by molding a styrene resin composition containing a syndiotactic polystyrene resin and a low dielectric filler having a dielectric constant of 5.5 F / m or less at a frequency of 10 GHz. The low dielectric filler is preferably mixed in a range of 1 to 50 parts by mass based on 100 parts by mass of the entire styrene resin composition.
[0059] The substrate as a laminate of a film of the resin molded body and a metal film according to the present invention can be produced by laminating a film obtained by molding the above-mentioned styrene-based resin composition and a metal film.
[0060] This application claims the benefit of priority based on Japanese Patent Application No. 2022-050817 filed on March 25, 2022. The entire contents of the specification of Japanese Patent Application No. 2022-050817 are incorporated herein by reference. [Example]
[0061] The present invention will be described in more detail below with reference to the following examples, but the present invention is not limited to the following examples and can be implemented with modifications within the scope of the above and the following gist, which are all included in the technical scope of the present invention.
[0062] The following materials were used in Examples and Comparative Examples. ·Syndiotactic polystyrene resin "XAREC 130ZC" manufactured by Idemitsu Kosan Co., Ltd. Low dielectric filler Low dielectric glass "HTD-09100T" manufactured by TOCHU Co., Ltd. "HTD-09100T" is a round diameter glass with a silane-based surface treatment. The dielectric constant of "HTD-09100T" at a frequency of 10GHz is 4.2F / m. The SiO2 content of "HTD-09100T" is 51% by mass, the B2O3 content is 24% by mass, the CaO content is 8.7% by mass, and the SrO content is 0.02% by mass. Hollow glass microspheres “Q-CEL (registered trademark) 5020FPS” manufactured by Potters-Ballotini Co., Ltd. The dielectric constant of “Q-CEL (registered trademark) 5020FPS” at a frequency of 10 GHz is 2.6 F / m. Hollow glass microspheres “Q-CEL (registered trademark) 7040S” manufactured by Potters-Ballotini Co. The dielectric constant of “Q-CEL (registered trademark) 7040S” at a frequency of 10 GHz is 1.3 F / m. "Advancell EM501" expanded beads manufactured by Sekisui Chemical Co., Ltd. The dielectric constant of "Advancell EM501" after expansion at a frequency of 10 GHz is 1.0 F / m. High dielectric inorganic filler "EPH80M-01N" manufactured by Nippon Electric Glass Co., Ltd. "EPH80M-01N" is a round diameter glass with a dielectric constant of 6.5F / m at a frequency of 10GHz. "HTD-09100T" contains 56% SiO2, 5.7% B2O3, 21% CaO, and 0.18% SrO.
[0063] (Example 1) Resin composition 1 was prepared by mixing 78 parts by mass of "XAREC 130ZC" as a syndiotactic polystyrene resin and 22 parts by mass of "HTD-09100T" as a low dielectric filler.
[0064] (Comparative Example 1) A resin composition 11 was prepared under the same conditions as in Example 1 except that 22 parts by mass of "EPH80M-01N" as a high dielectric inorganic filler was used instead of the low dielectric filler used in Example 1.
[0065] (Example 2) Resin composition 2 was prepared by mixing 78 parts by mass of "XAREC 130ZC" as a syndiotactic polystyrene resin, 11 parts by mass of "Q-CEL (registered trademark) 5020FPS" as a low dielectric filler, and 11 parts by mass of "EPH80M-01N" as a high dielectric inorganic filler.
[0066] (Example 3) Resin composition 3 was prepared by mixing 78 parts by mass of "XAREC 130ZC" as a syndiotactic polystyrene resin and 22 parts by mass of "Q-CEL (registered trademark) 5020FPS" as a low dielectric filler.
[0067] (Example 4) Resin composition 4 was prepared by mixing 78 parts by mass of "XAREC 130ZC" as a syndiotactic polystyrene resin and 22 parts by mass of "Q-CEL (registered trademark) 7040S" as a low dielectric filler.
[0068] (Example 5) Resin composition 5 was prepared by mixing 84 parts by mass of "XAREC 130ZC" as a syndiotactic polystyrene resin, 15 parts by mass of "HTD-09100T" as a low dielectric filler, and 1 part by mass of "Advancell EM501" as a low dielectric filler.
[0069] (Example 6) Resin composition 6 was prepared by mixing 84 parts by mass of "XAREC 130ZC" as a syndiotactic polystyrene resin, 15 parts by mass of "Q-CEL (registered trademark) 5020FPS" as a low dielectric filler, and 1 part by mass of "Advancell EM501" as a low dielectric filler.
[0070] (Example 7) Resin composition 7 was prepared by mixing 84 parts by mass of "XAREC 130ZC" as a syndiotactic polystyrene resin, 15 parts by mass of "Q-CEL (registered trademark) 7040S" as a low dielectric filler, and 1 part by mass of "Advancell EM501" as a low dielectric filler.
[0071] The resin composition (resin composition 1 to 7, 11) prepared according to the above-mentioned embodiment or comparative example is supplied to a co-directional twin-screw extruder with a screw diameter of 50 mm. After extrusion, it is water-cooled, granulated, and resin pellets are manufactured. The obtained resin pellets are supplied to a co-directional single-screw extruder with a screw diameter of 50 mm, and cooled using a cooling contact roller to manufacture a rod-shaped test material (0.3mmΦ×300mm) or a sheet-shaped test material (length 130mm×width 100mm×thickness 0.3mm) as a resin molding. As a cooling contact roller, a roller with a surface roughness Rz of 30μm is used, and the temperature of the cooling contact roller is 25°C. The composition of the test material is shown in Table 1 below. In Table 1 below, the mass ratio of the syndiotactic polystyrene resin to the low dielectric filler (low dielectric filler / syndiotactic polystyrene resin) and the mass ratio of the low dielectric filler to the high dielectric inorganic filler (high dielectric inorganic filler / low dielectric filler) contained in the test material are combined and represented.
[0072] (Example 8) Using the resin composition 1 prepared in Example 1, a rod-shaped test material (0.3 mm Φ × 300 mm) or a sheet-shaped test material (130 mm long × 100 mm wide × 0.3 mm thick) was manufactured under the same conditions as above except that a cooling touch roller having a surface roughness Rz of 110 μm was used. The component composition of the test material is shown in Example 8. It should be noted that the component composition of Example 8 is the same as that of Example 1.
[0073] (Example 9) The rod-shaped test material (0.3 mm Φ × 300 mm) and the sheet-shaped test material (130 mm long × 100 mm wide × 0.3 mm thick) prepared according to Example 1 were heat-set at 200°C × 1 hour using a dryer. The composition of the test material is shown in Example 9. It should be noted that the composition of Example 9 is the same as that of Example 1.
[0074] (Example 10) The rod-shaped test material (0.3 mm Φ × 300 mm) and the sheet-shaped test material (130 mm long × 100 mm wide × 0.3 mm thick) prepared according to Example 1 were heat-set at 170° C. × 1 hour using a dryer. The composition of the test material is shown in Example 10. It should be noted that the composition of Example 10 is the same as that of Example 1.
[0075] (Example 11) The rod-shaped test material (0.3 mm Φ × 300 mm) and the sheet-shaped test material (130 mm long × 100 mm wide × 0.3 mm thick) manufactured according to Example 1 were heat-set at 150° C. × 1 hour using a dryer. The composition of the test material is shown in Example 11. It should be noted that the composition of Example 11 is the same as that of Example 1.
[0076] (Example 12) Using the resin composition 1 prepared in Example 4, a rod-shaped test material (0.3 mm Φ × 300 mm) or a sheet-shaped test material (length 130 mm × width 100 mm × thickness 0.3 mm) was manufactured under the same conditions as above except that a cooling touch roller having a surface roughness Rz of 110 μm was used. The component composition of the test material is shown in Example 12. It should be noted that the component composition of Example 12 is the same as that of Example 4.
[0077] (Example 13) The rod-shaped test material (0.3 mm Φ × 300 mm) and the sheet-shaped test material (130 mm long × 100 mm wide × 0.3 mm thick) manufactured according to Example 4 were heat-set at 150° C. × 1 hour using a dryer. The composition of the test material is shown in Example 13. It should be noted that the composition of Example 13 is the same as that of Example 4.
[0078] To the sheet-like test material of gained, the heating crystallization temperature, the cooling crystallization temperature and the crystallinity are calculated by DSC measurement analysis. In addition, for the rod-like test material of gained, the dielectric constant under the frequency of 10GHz is measured, and the dielectric properties are evaluated. In addition, for the rod-like test material of gained, the dielectric loss tangent under the frequency of 10GHz is measured. In addition, the film forming property when the resin particles consisting of the resin composition prepared according to the embodiment or the comparative example are processed into the sheet-like test material is evaluated. To the sheet-like test material of gained, heat resistance is evaluated, the linear expansion coefficient is measured, and the linear expansion characteristics are evaluated. In addition, the L value and the gloss value of the sheet-like test material of gained are measured.
[0079] (Crystallization temperature at rising temperature (Tc1), crystallization temperature at falling temperature (Tc2), degree of crystallinity) The temperature of the rod-shaped test material was determined by using a differential scanning calorimeter (DSC) "TAS100 Thermal Analysis System" manufactured by TA Instruments. A test piece of 5.0±0.3 mg cut from a rod-shaped test material was placed in an aluminum crucible and heated from room temperature to 320°C at a heating rate of 20°C / min, and the temperature of the crystallization (Tc1) was determined. Further, after reaching 320°C and holding for 5 minutes, it was cooled at a cooling rate of 20°C / min, and the temperature of the crystallization (Tc2) was determined. The temperature of the crystallization (Tc1) and the temperature of the crystallization (Tc2) are the temperatures of the most parts of their respective peaks. The degree of crystallization is calculated based on the ratio of the latent heat of the melting point to the latent heat of the crystallization temperature (Tc2). The calculation results are shown in Table 1 below.
[0080] (Dielectric properties) A test piece of 0.3 mm Φ × 100 mm was cut from a rod-shaped test material (0.3 mm Φ × 300 mm), and the dielectric constant (εr) and dielectric loss tangent (Df) at a frequency of 10 GHz were measured by the resonant cavity perturbation method. When measuring the dielectric constant and dielectric loss tangent, the "Precision LCR Meter" manufactured by Agilent Technologies was used. The measurement results are shown in Table 1 below. In addition, based on the measured dielectric constant (εr), the dielectric properties were evaluated according to the following criteria. The evaluation results are shown in Table 1 below. (Evaluation Criteria) Dielectric properties pass (○): Dielectric constant (εr) is 3.2 F / m or less. Dielectric properties unqualified (×): Dielectric constant (εr) exceeds 3.2F / m.
[0081] The dielectric loss tangent was 0.002 or less and was considered acceptable, whereas the dielectric loss tangent was considered unacceptable if it exceeded 0.002.
[0082] (Film-forming property) When the obtained resin pellets were supplied to a single screw extruder to produce a sheet-like test material of 130 mm in length × 100 mm in width × 0.3 mm in thickness, the case where the sheet-like test material could be produced was evaluated as having a qualified film-forming property (○), and the case where the sheet-like test material could not be produced was evaluated as having an unqualified film-forming property (×). It should be noted that when the film-forming property was unqualified, the subsequent physical property measurement and evaluation were not performed.
[0083] (Heat resistance) A test piece of 35 mm in length × 5 mm in width × 0.3 mm in thickness is cut out from a sheet-like test material (130 mm in length × 100 mm in width × 0.3 mm in thickness), and the obtained test piece is immersed in a solder bath heated to 260°C for 120 seconds. Visually observe the morphology of the test piece before and after immersion to confirm whether there is deformation. The case where no deformation is confirmed before and after immersion is evaluated as qualified heat resistance (◎), the case where there is slight deformation but it can still be fully used is evaluated as qualified heat resistance (◎~○), the case where there is a small amount of deformation but it can still be used is evaluated as qualified heat resistance (○), and the case where obvious deformation is confirmed and it cannot be used is evaluated as unqualified heat resistance (×). The evaluation results are shown in Table 1 below.
[0084] (Linear expansion characteristics) A test piece of 50 mm long × 50 mm wide × 0.3 mm thick was cut out from a sheet-like test material (130 mm long × 100 mm wide × 0.3 mm thick), and the linear expansion coefficient was measured using a thermomechanical analyzer ("TM7000" applicable film manufactured by Hitachi High-tech Science Co., Ltd.). The measurement temperature range is 30°C to 200°C. The measurement results are shown in Table 1 below. In addition, the case where the linear expansion coefficient is less than 200 ppm is evaluated as a qualified linear expansion characteristic, and the case where the linear expansion coefficient exceeds 200 ppm is evaluated as an unqualified linear expansion characteristic. The evaluation results are shown in Table 1 below.
[0085] (L value) A test piece of 50 mm long, 50 mm wide and 0.3 mm thick was cut from a sheet-like test material (130 mm long, 100 mm wide and 0.3 mm thick) as a test piece for evaluation. A "TC-1500MC-88" manufactured by Tokyo Denshoku Co., Ltd. was used as a colorimeter, and light source C was used to irradiate the center of the test piece for evaluation, and the L value of the Lab color system was measured. The measurement results are shown in Table 1 below.
[0086] (Gloss value) A test piece of 70 mm long, 70 mm wide and 0.3 mm thick was cut from a sheet-like test material (130 mm long, 100 mm wide and 0.3 mm thick) as a test piece for evaluation. The gloss value at a surface angle of 60° was measured using a "VG-2000" manufactured by Nippon Denshoku Industries Co., Ltd. as a gloss meter. The measurement results are shown in Table 1 below.
[0087] [Table 1-1]
[0088] [Table 1-2]
[0089] The following investigations can be conducted based on Table 1. Examples 1 to 13 are resin molded bodies that meet the necessary conditions specified in the present invention, have low dielectric constants, and can have both low dielectric properties and heat resistance. In particular, when comparing Example 1 with Example 8, and Example 4 with Example 12, it can be seen that by reducing the surface roughness Rz of the cooling contact roller, the L value and gloss value of the sheet-like test material can be improved, and the appearance is good. When comparing Example 1 with Examples 9 to 11, and Example 4 with Example 13, it can be seen that by applying heat setting to the resin molded body, the heat resistance is further improved. When comparing Examples 9 to 11, it can be seen that the higher the temperature of the heat setting applied to the resin molded body, the higher the heat resistance is improved and the smaller the linear expansion coefficient. On the other hand, Comparative Example 1 is an example of not using a low dielectric filler with a dielectric constant of less than 5.5F / m at a frequency of 10GHz, but using a high dielectric inorganic filler with a dielectric constant of more than 5.5F / m and a dielectric constant of 6.5F / m at a frequency of 10GHz, and the dielectric constant of the resin molded body is increased, and the transmission loss increases.
Claims
1. A styrene resin molded body, comprising a syndiotactic polystyrene resin, and containing 1 to 50 parts by mass of a low dielectric filler having a dielectric constant of 5.5 F / m or less at a frequency of 10 GHz, based on 100 parts by mass of the entire resin molded body. 2 . The styrene resin molded article according to claim 1 , wherein the low dielectric filler is low dielectric glass.
3. The styrene resin molded article according to claim 2, wherein the low dielectric glass contains 10 to 30% by mass of B2O3. 4 . The styrene resin molded article according to claim 1 , further comprising 50 parts by mass or less of a high dielectric inorganic filler having a dielectric constant exceeding 5.5 F / m at a frequency of 10 GHz, based on 100 parts by mass of the entire resin molded article. The styrene resin molded article according to claim 1 , which has a heating crystallization temperature of 180° C. or less.
6. The styrene resin molded article according to claim 1, which has a cooling crystallization temperature of 260°C or lower and a crystallinity of 30% or higher.
7. The styrene resin molded article according to claim 1, which has a linear expansion coefficient of 200 ppm or less.
8. The styrene resin molded article according to claim 1, which has an L value of 70 or more and a gloss value of 30% or more. 9 . The styrene resin molded article according to claim 1 , which is used for electronic equipment or communication equipment used in a high frequency band of 1 GHz or more. 10 . The styrene resin molded article according to claim 1 , which is a film. 11 . A substrate which is a laminate of the styrene-based resin molded article according to claim 1 and a metal film as a film.
Citation Information
Patent Citations
Styrene-based resin composition, film, circuit-board and molded product
JP2004323650A
Low-dielectric / heat-resistant resin composition, and molded product, copper-clad laminate and flexible printed wiring board using the composition
JP2005213317A
Foam, foam sheet, product, and foam production method
JP2022050817A