Copper foil for flexible printed circuit board, copper-clad laminate using same, flexible printed circuit board, and electronic device
By optimizing the composition and heat treatment process of copper foil to ensure uniform metal structure, the problem of unstable circuit bottom width in micro circuits is solved, and the effect of linear and high-density configuration of circuits is achieved.
Patent Information
- Application Number
- CN202380029551.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-07-14
- Filing Date
- 2023-03-15
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art is difficult to maintain the stability of the circuit bottom width in the fine circuit, resulting in the circuit being easily in contact with adjacent circuits, affecting the high-density configuration and the overall impedance integration of the circuit.
By using Cu copper foil with a purity of 99.96% or more, and EBSD measurement was performed after heat treatment at 300°C×30 minutes, the average crystal particle size of the copper foil was less than 5.0 μm and the standard deviation was less than 3.0 μm, and the addition was performed with 10-50 ppm. Elements optimize the metal structure uniformity of copper foil, thereby improving the linearity of the etching circuit.
It realizes that the circuit is linear and suitable for micro circuits is flexible printed substrate, which reduces the contact between the circuit and adjacent circuits, and improves the overall performance and density of the circuit.
Smart Images

Figure CN118922570A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a copper foil suitable for use in wiring members such as a flexible printed circuit board, a copper-clad laminate using the same, a flexible wiring board, and an electronic device. Background Art
[0002] As a circuit substrate for electronic equipment, a flexible printed circuit board (flexible wiring board, hereinafter referred to as "FPC") is widely used. FPC is formed by etching a copper clad laminate (hereinafter referred to as CCL) formed by laminating copper foil and resin to form wiring, and then covering it with a resin layer called a cover layer. The resin bonded to the CCL can be polyimide, liquid crystal polymer, PTFE, but is not limited to these.
[0003] In this way, the copper-clad laminate undergoes a process of printing the circuit by applying a resist and performing an exposure step in order to form the target circuit, and then etching to remove unnecessary portions of the copper layer. However, there is a problem that when the circuit is formed by etching, the circuit will not become as wide as the shielding pattern pre-formed on the surface.
[0004] This is because the copper circuit formed by etching is etched gradually from the surface of the copper layer downward, that is, toward the resin layer (causing collapse).
[0005] Therefore, a technology for reducing this "collapse" is being developed (Patent Document 1).
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2011-216528. Summary of the invention
[0009] [Problems to be solved by the invention]
[0010] Furthermore, as electronic devices become smaller, thinner, and more high-performance, high-density FPC packaging is required. In order to package FPCs at a high density, the circuit needs to be miniaturized, but in order to maintain impedance integrity in a miniaturized circuit, it is important that the circuit width is fixed to the entire circuit. The reason is that when the circuit width is not fixed to the entire circuit, the circuit will be close to (contact) the adjacent circuit, and there is a concern that it will become defective.
[0011] Furthermore, as described above, since the circuit width tends to spread on the resin layer side (bottom side), the bottom side is more likely to contact with the adjacent circuit, and it becomes more important to keep the circuit width (bottom width) on the bottom side fixed in the entire circuit. This defect is more likely to occur in the case of a fine circuit with a bottom width of 35μm or less.
[0012] However, as described in the above-mentioned Patent Document 1, although a technique for reducing the difference (collapse) between the top width and the bottom width of a circuit is disclosed, no technique focusing on the bottom width is found.
[0013] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a copper foil for a flexible printed circuit board which has excellent circuit linearity and is suitable for a fine circuit, a copper-clad laminate using the same, a flexible printed circuit board, and an electronic device.
[0014] [Technical means to solve the problem]
[0015] The inventors of the present invention have conducted various studies and found that in order to improve the linearity of the circuit formed by etching copper foil, it is important that the metal structure of the copper foil is close to uniform, in other words, the size of the crystal grains is uniform (the average crystal grain size is small). This is believed to be because if the average crystal grain size is small, the chemical reaction (etching reaction) during circuit formation caused by etching occurs uniformly.
[0016] That is, the copper foil for a flexible printed circuit board of the present invention is a rolled copper foil containing 99.96% by mass or more of Cu, with the remainder being composed of inevitable impurities, and when subjected to a heat treatment at 300° C. for 30 minutes, an EBSD measurement is performed on a measurement field of view of 150 μm×150 μm on the rolled surface of the rolled copper foil, and the average crystal grain size when an orientation difference of 5° or more is regarded as a grain boundary is 5.0 μm or less.
[0017] In the copper foil for a flexible printed circuit board of the present invention, it is preferred that the standard deviation of the crystal grain size obtained by the EBSD measurement is 3.0 μm or less.
[0018] The copper foil for a flexible printed circuit board of the present invention is preferably made of refined copper specified in JIS-H3100 (C1100) or oxygen-free copper specified in JIS-H3100 (C1020).
[0019] The copper foil for a flexible printed circuit board of the present invention preferably contains 10 to 50 mass ppm of P.
[0020] The copper-clad laminate of the present invention is obtained by laminating the above-mentioned copper foil for a flexible printed circuit board and a resin layer.
[0021] The flexible printed circuit board of the present invention is formed by forming a circuit on the copper foil in the copper-clad laminate.
[0022] The electronic device of the present invention is formed by using the above-mentioned flexible printed circuit board.
[0023] [Effects of the Invention]
[0024] According to the present invention, a copper foil for a flexible printed circuit board having excellent circuit linearity and suitable for a fine circuit can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] [ Figure 1 ] is a diagram showing the bottom width w of the circuit formed by etching.
[0026] [ Figure 2 ] is a top view showing a method of measuring the bottom width w of a circuit multiple times.
[0027] [ Figure 3 ] is a diagram showing an exposure mask used to etch a straight line circuit when evaluating the linearity of the circuit.
[0028] [ Figure 4 ] is a schematic diagram showing the state of etching progress in a straight line circuit.
[0029] [ Figure 5 ] is a schematic diagram showing the mechanism by which circuit linearity decreases when the metal structure is uneven (the size of the grains is inconsistent). DETAILED DESCRIPTION
[0030] Hereinafter, the embodiment of the copper foil of the present invention will be described. In addition, in the present invention, % represents mass % unless otherwise specified.
[0031] <Composition>
[0032] The copper foil of the present invention contains 99.96% by mass or more of Cu, and the remainder is composed of inevitable impurities. It is preferred if 10 to 50 ppm by mass of P is contained as an additive element. Here, if Cu is in the range of 99.96% by mass or more, in order to improve the mechanical properties of the copper foil, the copper foil may also contain trace amounts of Ag, Sn, Zr, etc.
[0033] If P is contained as an additive element, the metal structure (crystal grain size) tends to become uniform, and the bottom width of the circuit after etching tends to become constant. However, if the P content exceeds 50 mass ppm (0.005 mass%), the conductivity decreases, making it unsuitable for flexible printed circuit boards.
[0034] The copper foil of the present invention may be made of refined copper specified in JIS-H3100 (C1100) or oxygen-free copper of JIS-H3100 (C1020), or may be oxygen-free copper or refined copper containing trace amounts of Ag, Sn, Zr, etc., and these compositions may contain 10 to 50 mass ppm of P as an additive element.
[0035] The analysis of phosphorus concentration was carried out by using the phosphomolybdic acid blue absorption measurement method using phosphomolybdic acid (mollide acid) extraction specified in JIS H 1058 (phosphorus quantitative method in copper and copper alloys) (P concentration: applicable to 0.0005% to 0.01%).
[0036] <Average crystal grain size>
[0037] When the rolled copper foil was heat treated at 300°C for 30 minutes, EBSD measurement was performed on the rolled surface after the heat treatment with a measurement field of 150 μm×150 μm. The average crystal grain size was 5.0 μm or less when the orientation difference of 5° or more was regarded as the grain boundary.
[0038] The average crystal grain size is calculated by crystal orientation analysis in EBSD (Electron Back Scatter Diffraction) measurement.
[0039] The actual measurement was carried out by electrolytically polishing the sample surface and then observing it using SEM-EBSD (JSM-IT500HR, TSL EDAX SCAN GENERATOR-II, TSL OIM DATA COLECTION 7, JEOL Ltd.) under the following conditions.
[0040] In addition, EBSD measurement may be performed on a sample plate (150 mm×150 mm) cut out from the copper foil after the heat treatment.
[0041] WD: 15.0mm or 16.0mm
[0042] Camera elevation angle: 2.7 degrees
[0043] Sample tilt angle: 70.0 degrees
[0044] Camera azimuth: 0.0 degrees
[0045] Accelerating voltage: 15.0 kV
[0046] Probe current: 9.5nA
[0047] SS-CCD camera: 8×8 grid
[0048] Gain: 300-350 (Pattern brightness: 0.90-0.95)
[0049] Exposure time: 4ms
[0050] Background integration count: 20 times
[0051] Observation magnification: 600 times
[0052] Observation field: 150μm×150μm
[0053] ·Step width: 0.5μm
[0054] Scanning pattern: Hexagonal grid
[0055] Phase list: Copper.
[0056] The analysis of the obtained measurement data was performed using OIM Analysis Ver8.0 x64 Advanced package under the following conditions.
[0057] ·Perform Crean Up using the grain expansion method once (grain tolerance angle: 5, minimum grain size: 2 points, multiple rows: 1, iteration score: 0.25)
[0058] · Grains at the edge of the EBSD image are not calculated
[0059] · The average value and standard deviation of the crystal grain size (Diameter) were calculated using the area fraction method.
[0060] Here, in the area fraction method, the average value of the crystal grain size is calculated by multiplying the ratio of the area of each grain to the total area of the observation field by the average value of each area value. That is, when even one coarse grain is observed in the observation field, the average crystal grain size tends to be larger than the number method, and the small average crystal grain size in the area fraction method indicates that the size of the crystal grains is uniform and small.
[0061] It is believed that when the average crystal grain size, especially the average crystal grain size by the area fraction method, is 5.0 μm or less, the metal structure of the copper foil becomes nearly uniform (the size of the crystal grains is uniform), and the chemical reaction (etching reaction) during circuit formation by etching occurs uniformly.
[0062] <Circuit linearity>
[0063] After the copper foil was surface treated, a sample plate (150 mm × 150 mm) was cut out and subjected to heat treatment to form a copper-clad laminate. A straight line circuit was formed from the copper foil side of the copper-clad laminate under the following etching conditions (refer to Figure 2), when the bottom width w of the circuit is measured multiple times, it is better if σ / Aw represented by the standard deviation σ(μm) of the bottom width w(μm) and the average value Aw(μm) of the bottom width w is less than 0.03. The reason is that if σ / Aw is less than 0.03, it is known from experience that there is a tendency for the circuit to have excellent linearity.
[0064] Etching conditions:
[0065] The composition of the etching solution: CuCl2-2H2O=3mol / L (specific gravity 1.24), HCl=4mol / L, liquid temperature=50°C, etching solution spray pressure=0.22MPa, the rolled copper foil of the shielded circuit portion is etched to form a circuit.
[0066] σ / Aw is calculated by measuring the actual bottom width w of the circuit formed by etching multiple times (preferably 10 or more locations, more preferably 50 locations, and even more preferably 100 locations every 30 μm in the long side direction of the circuit) to obtain σ and Aw.
[0067] Specifically, if Figure 1 As shown, the circuits 21 and 22 formed by etching the copper foil are extended from the surface toward the bottom (resin layer 4 side (bottom side)), and the circuit width (bottom width) w on the bottom side is measured multiple times. Here, the symbol wt is the circuit width (top width) on the surface (top) side.
[0068] Furthermore, if Figure 2 As shown, the circuits 21 and 22 can be measured at specific measurement points, such as 50 locations of the circuit widths w1, w2, w100, w101, w102, w200, etc. The measurement can also be performed on one circuit.
[0069] When σ / Aw is less than 0.03, the variation in the bottom width w is small, indicating excellent circuit linearity. In particular, it is preferred that the circuit linearity is excellent even when the bottom width w is in the range of 10 to 35 μm.
[0070] The shielding of the circuit portion of the copper foil can be formed by, for example, using a known method of using a photoresist (dry film resist, etc.) to leave the resist only on the portion remaining as the circuit through a mask. As a dry film resist, for example, RY-5107 (thickness 7 μm) manufactured by Hitachi Chemical can be used.
[0071] Here, Figure 3 This is an exposure mask used to etch a straight line circuit when evaluating the linearity of the circuit. There are 10 types of resist / space patterns in the exposure mask, and they are Figure 3The design is that the space is wider on the left side (number 10 side) and narrower on the right side. After all patterns are sequentially exposed, developed, etched, and dry film stripped, a circuit with a L / S close to the target (L / S = 10 / 40 to 30 / 20) is selected from all patterns for evaluation using SEM.
[0072] The thickness of the copper foil is preferably 17 μm or less in terms of the nominal thickness specified in JIS C 6515. The thinner the thickness, the smaller the stress applied to the copper foil, which helps improve the bending property and also helps to make portable devices smaller, thinner, and lighter.
[0073] <Manufacturing>
[0074] The copper foil of the present invention can be produced, for example, as follows: First, P is added to a copper ingot as necessary, and the ingot is melted and cast, and then hot rolling, cold rolling, and annealing are repeated to produce a foil.
[0075] Here, intermediate annealing at a predetermined cooling rate may be performed during the cold rolling, and oxide scale generated during the intermediate annealing may be removed. After intermediate cold rolling, final annealing and final cold rolling may be performed to obtain a foil having a target final thickness.
[0076] The maximum temperature of the intermediate annealing can be set to 350 to 500° C. The cooling rate of the intermediate annealing is preferably 50 to 150° C. / h from the maximum temperature TM (° C.) in the intermediate annealing to a temperature of (TM-200)° C.
[0077] As mentioned above, if the cooling rate of the intermediate annealing is set to 50 to 150°C / h, the cooling rate becomes slower than the general conditions. Moreover, the slower the cooling rate of the intermediate annealing, the smaller the temperature gradient in the material (the temperature difference between the first cooled part and the last cooled part becomes smaller), thereby making the metal structure more uniform (the size of the grains is uniform), and the average crystal grain size becomes smaller when the foil of the final thickness is heat treated. As a result, it is believed that the chemical reaction (etching reaction) during the circuit formation caused by etching occurs uniformly, so the circuit linearity is improved.
[0078] This is because, as described above, it means that the smaller the crystal grain size according to the area fraction method is, the more uniform the size of the crystal grains is, and the smaller the grain size of each crystal grain is.
[0079] Figure 4 , Figure 5 This is a mechanism that indicates that the more uniform the metal structure (the more uniform the grain size), the better the circuit linearity.
[0080] like Figure 4As shown in the figure, etching is the process where the etching liquid penetrates into the copper foil from the part without resist (equivalent to the space between the straight lines) and expands, while etching expands from the space to the left and right of the copper foil. Figure 1 As shown, etching (circuit) spreads from the surface toward the bottom (resin layer side (bottom side)).
[0081] Here, if Figure 5 As shown in (a), when the metal structure is not uniform (the size of the grains is not uniform), Figure 1 The bottom width w of the circuits 21 and 22 shown in FIG. Figure 5 In (a), the edges of the circuits 21 and 22 are not straight lines but are curved in an undulating manner).
[0082] The reason is believed to be Figure 5 As shown in (b), for example, within a field of view of 150μm×150μm, if the grains of the copper foil on the circuit 21 side are large and the grains of the copper foil on the circuit 22 side are small, the metal structure is not uniform (the grain sizes are inconsistent), and the etching speed on the circuit 21 side with large grains increases, and the etching amount changes between the parts with small grains, and even the unevenness of the bottom width w increases.
[0083] Furthermore, Figure 5 In (b), since the etching rates are different in the crystal grains and the crystal grain boundaries, if the crystal grain sizes are not uniform, the etching rate will vary greatly locally. Furthermore, in the etching solution of this experiment, the etching rate of the crystal grain boundaries is slower than that of the crystal grains, but the opposite situation also exists.
[0084] If the standard deviation of the crystal grain size obtained by the above EBSD measurement is less than 3.0 μm, the size of the grains is further consistent, so it is better. The method for determining the standard deviation of the crystal grain size is as described in the above EBSD measurement. For the measurement results, by the area fraction method, not only the average value (average crystal grain size) of the crystal grain size can be calculated, but also the standard deviation can be calculated.
[0085] <Copper clad laminate and flexible printed circuit board>
[0086] Furthermore, the copper foil of the present invention can be polymerized by (1) casting a resin precursor (e.g., a polyimide precursor called varnish) and applying heat, and (2) laminating a base film on the copper foil of the present invention using a thermoplastic adhesive of the same type as the base film, thereby obtaining a copper clad laminate (CCL) consisting of two layers of copper foil and a resin substrate. Furthermore, by laminating a base film coated with an adhesive on the copper foil of the present invention, a copper clad laminate (CCL) consisting of three layers of copper foil, a resin substrate, and an adhesive layer therebetween can be obtained. When manufacturing these CCLs, the copper foil is heat-treated and recrystallized.
[0087] A circuit is formed on these by using a photolithography technique, and the circuit is plated as necessary, followed by laminating a cover layer film, thereby obtaining a flexible printed circuit board (flexible wiring board).
[0088] Therefore, the copper-clad laminate of the present invention is formed by laminating copper foil and resin layers. In addition, the flexible printed circuit board of the present invention is formed by forming a circuit on the copper foil of the copper-clad laminate.
[0089] Examples of the resin layer include PET (polyethylene terephthalate), PI (polyimide), LCP (liquid crystal polymer), and PEN (polyethylene 2,6 naphthalate), but are not limited thereto. In addition, these resin films may be used as the resin layer.
[0090] As a lamination method of the resin layer and the copper foil, the material to be the resin layer may be applied to the surface of the copper foil and heated to form a film. In addition, a resin film may be used as the resin layer, and the following adhesive may be used between the resin film and the copper foil, or the resin film may be thermally pressed onto the copper foil without using an adhesive. However, it is preferred to use an adhesive in order to avoid applying excess heat to the resin film.
[0091] When a film is used as the resin layer, the film can be laminated on the copper foil via an adhesive layer. In this case, it is preferred to use an adhesive having the same composition as the film. For example, when a polyimide film is used as the resin layer, a polyimide-based adhesive is also preferably used as the adhesive layer. Furthermore, the polyimide adhesive referred to herein refers to an adhesive containing an imide bond, and also includes polyetherimide and the like.
[0092] The present invention is not limited to the above-described embodiment. Furthermore, the copper alloy in the above-described embodiment may contain other components as long as the effects of the present invention are exhibited.
[0093] For example, the surface of the copper foil may be subjected to a roughening treatment, a rust-proof treatment, a heat-resistant treatment, or a surface treatment in which these treatments are combined.
[0094] [Example]
[0095] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples.
[0096] Ingots are made using electrolytic copper in a non-oxidizing environment. The proportion of copper contained in the ingot is 99.96% by mass or more. After the ingot is homogenized and annealed at above 900°C, hot rolling and cold rolling are performed. During the cold rolling, an intermediate annealing with a maximum temperature of 400°C is performed, and the cooling rate of the intermediate annealing is set to the value in Table 1, and the temperature is cooled to 200°C lower than the maximum temperature. The cooling rate of the embodiment is calculated based on the measured data of the material temperature when annealing a material different from the embodiment. After removing the oxide scale generated during the intermediate annealing and performing intermediate cold rolling, the final annealing and final cold rolling are performed to obtain the target foil with a final thickness of 12μm. Furthermore, for the comparative example, the cooling rate of the intermediate annealing to a temperature 200°C lower than the maximum temperature is obtained by heat transfer simulation, which is recorded in Table 1.
[0097] The obtained foil was subjected to a heat treatment of 300°C for 30 minutes in an atmospheric environment to obtain a copper foil sample. Specifically, in order to prevent oxidation, the copper foil sample was sandwiched between two C7025 plates of 30 mm in width, 130 mm in length, and 0.15 mm in thickness. After packaging with A4-sized annealed C1100, the door of a high-temperature hot air dryer at 300°C was opened and put into the dryer. After 30 minutes, the door was opened for recovery and the copper foil sample was taken out. The heat-treated copper foil simulated the state of heat treatment during the lamination of CCL. After electrolytically polishing the rolled surface of the heat-treated copper foil, EBSD measurement was performed on the measurement field of 150 μm × 150 μm to obtain the average value (average crystal grain size) and standard deviation of the crystal grain size when the orientation difference of 5° or more is regarded as the grain boundary. The conditions for EBSD measurement are as described above.
[0098] After the foil obtained by the final cold rolling was surface treated, 25 μm of UPIREX VT (manufactured by Ube Industries, Ltd.) was laminated, and heat treated at 300°C × 30 minutes using a heating press to form a copper-clad laminate. Then, the circuit part of the copper foil was masked by photoetching using a dry film resist (product name RY-5107 manufactured by Hitachi Chemical, thickness 7 μm), and dry film patterning with a L+S pitch of 50 μm was performed. The development, etching, and stripping of the resist were performed using the "Development, Etching, Stripping Production Line" (device name: DERM) of Suntec System Co., Ltd. The etching conditions were as described in the above "<Circuit Linearity>".
[0099] <Evaluation of circuit linearity>
[0100] The above etching conditions were actually measured. The etching time was changed for each embodiment and each comparative example in a manner close to the target L / S (L / S = 10 / 40 to 30 / 20). As a result, the average value Aw of the bottom width w became the value shown in Table 1. The average value Aw represents L of L / S. In addition, "50μm-average value Aw" represents S of L / S. For each embodiment and each comparative example, the bottom width w of each circuit was set as shown in Table 1. Figure 2 50 points were measured and the average value Aw was calculated.
[0101] In addition, each Example changes the etching time within the range of 36 to 54 seconds for the same copper foil. Similarly, each Comparative Example changes the etching time within the range of 36 to 54 seconds for the same copper foil.
[0102] The obtained results are shown in Table 1. Here, the P concentration of Examples 1 to 7 was in the range of 10 to 50 mass ppm, and the P concentration of Comparative Examples 1 to 7 was less than 10 ppm. The analysis of the P concentration was performed by the above-mentioned method.
[0103]
[0104] When a flexible printed circuit board was produced using the copper foil of the example having an average crystal grain size of 5.0 μm or less, it was found that σ / Aw was less than 0.03, contact with adjacent circuits was almost not observed, and the circuit linearity was excellent.
[0105] On the other hand, when a flexible printed circuit board was produced using the copper foil of the comparative example having an average crystal grain size exceeding 5.0 μm, σ / Aw was found to be 0.03 or more, contact with adjacent circuits was seen everywhere, and the circuit linearity was poor.
Claims
1. A copper foil for a flexible printed circuit board, which is a rolled copper foil containing 99.96% by mass or more of Cu, the remainder of which is composed of inevitable impurities, When the rolled copper foil was heat treated at 300° C. for 30 minutes, EBSD measurement was performed on a measurement field of 150 μm×150 μm on the rolled surface, and the average crystal grain size was 5.0 μm or less when the orientation difference of 5° or more was regarded as a grain boundary.
2. The copper foil for a flexible printed circuit board according to claim 1, in, The standard deviation of the crystal grain size obtained by EBSD measurement was 3.0 μm or less. 3 . The copper foil for a flexible printed circuit board according to claim 1 , which is made of refined copper specified in JIS-H3100 (C1100) or oxygen-free copper specified in JIS-H3100 (C1020). The copper foil for a flexible printed circuit board according to any one of claims 1 to 3, comprising 10 to 50 mass ppm of P. 5 . A copper-clad laminate, comprising laminating the rolled copper foil for a flexible printed circuit board according to claim 1 and a resin layer.
6. A flexible printed circuit board, wherein a circuit is formed by using the rolled copper foil in the copper-clad laminate according to claim 5.
7. An electronic device using the flexible printed circuit board according to claim 6.