Adhesive film for semiconductor, dicing die bonding film, and method for manufacturing semiconductor device

By using a thermoset adhesive film and cutting film with specific shear viscosity in the range of 60 to 150°C, the problem of difficult to take into account both the ooze and the ooze in the semiconductor package is solved, and better ooze and ooze are achieved inhibition.

CN118922915APending Publication Date: 2024-11-08RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029854.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-03-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When manufacturing semiconductor packages, it is difficult to completely penetrate the semiconductor chip or wire with a low viscosity adhesive film, resulting in leakage problems. Especially when the chip or wire is large in size, it is difficult to take into account both the suppression and buried properties of leakage.

Method used

Adhesive film containing thermosetting components, and the shear viscosity at a frequency of 4.4 Hz in the range of 60 to 150°C is 2000 Pa·s or more and less. The cutting film and the cutting grain bonding film are used to improve bonding and burial. sex.

Benefits of technology

Effectively suppress leakage, while improving the buriedness of semiconductor packages, ensuring full buriedness of semiconductor chips or wires.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922915A_ABST
    Figure CN118922915A_ABST
Patent Text Reader

Abstract

An adhesive film for a semiconductor contains a thermosetting component. The adhesive film exhibits a shear viscosity at a frequency of 4.4 Hz at a minimum of 2000 Pa * s or more and a maximum of 200000 Pa * s or less in a range of 60 to 150 DEG C. The adhesive film may be used to adhere to a substrate while embedding other semiconductor chips. The adhesive film may be used to adhere the semiconductor chip to another semiconductor chip while embedding a portion or entirety of a wire connected to the other semiconductor chip.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive film for semiconductor, a dicing die bonding film, and a method for manufacturing a semiconductor device using the same. Background Art

[0002] Stacked MCP (MultiChip Package) has become popular, which realizes high capacity by stacking semiconductor chips in multiple layers. Examples of stacked MCP include wire-embedded type and chip-embedded type semiconductor packages. The structure of a semiconductor package in which the wire is embedded through an adhesive film is sometimes called FOW (Film Over Wire). The structure of a semiconductor package in which the semiconductor chip is embedded through an adhesive film is sometimes called FOD (Film Over Die). As an example of a semiconductor package using FOD, there is a semiconductor package having a controller chip arranged in the bottom layer and an adhesive film in which the controller is embedded (see Patent Document 1).

[0003] Previous technical literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2014-175459

[0006] Patent Document 2: Japanese Patent No. 5736899 Summary of the invention

[0007] Technical issues to be solved by the invention

[0008] In the manufacture of semiconductor packages having a FOD or FOW structure, it is required that the semiconductor chip or wire be fully embedded through the adhesive film. Although the adhesive film with low viscosity can show good embedding properties, sometimes a large amount of seepage of the adhesive film overflowing from the end of the semiconductor chip occurs. In particular, when the ratio of the volume of the embedded semiconductor chip or wire to the volume of the adhesive film is large, it is difficult to properly embed the semiconductor chip or wire, so it is difficult to balance the suppression of seepage and sufficient embedding properties. For example, in the case of embedding a controller chip with a thin adhesive film, the ratio of the volume of the embedded controller chip to the volume of the adhesive film is usually relatively large.

[0009] One aspect of the present invention relates to an adhesive film capable of improving embedding in a FOD or FOW while suppressing oozing out.

[0010] Means for solving technical problems

[0011] One aspect of the present invention relates to an adhesive film for semiconductors containing a thermosetting component, wherein the adhesive film can exhibit a shear viscosity at a frequency of 4.4 Hz of a minimum of 2,000 Pa·s or more and a maximum of 200,000 Pa·s or less in the range of 60 to 150° C.

[0012] Another aspect of the present invention relates to a dicing die bonding film including a dicing film and the adhesive film for a semiconductor provided on the dicing film.

[0013] Another aspect of the present invention relates to a method for manufacturing a semiconductor device, the method comprising the step of bonding a second semiconductor chip to a substrate on which a first semiconductor chip is mounted, via the adhesive film for a semiconductor, wherein the first semiconductor chip is embedded via the adhesive film.

[0014] Another aspect of the present invention relates to a method for manufacturing a semiconductor device, the method comprising the step of bonding a second semiconductor chip to a first semiconductor chip via the adhesive film for semiconductors. A wire is connected to the first semiconductor chip, and a part or the whole of the wire is buried via the adhesive film.

[0015] The present invention includes the following. [1]

[0017] An adhesive film for semiconductors, comprising a thermosetting component,

[0018] In the range of 60 to 150° C., the shear viscosity at a frequency of 4.4 Hz is shown to be at least 2,000 Pa·s and at most 200,000 Pa·s. [2]

[0020] The adhesive film for a semiconductor according to [1], which has a thickness of 50 to 150 μm. [3]

[0022] The adhesive film for a semiconductor according to [1] or [2] is used to bond a semiconductor chip to a substrate while embedding another semiconductor chip.

[0023] [3]'

[0024] The adhesive film for a semiconductor according to [1] or [2] is used for producing an adhesive film for a semiconductor that bonds a semiconductor chip to a substrate while embedding another semiconductor chip. [4]

[0026] The adhesive film for a semiconductor according to [1], which has a thickness of 25 to 80 μm. [5]

[0028] The adhesive film for a semiconductor according to [1] or [4] is used to bond a semiconductor chip to another semiconductor chip while burying a part or the whole of a wire connected to the other semiconductor chip.

[0029] [5]'

[0030] The adhesive film for a semiconductor according to [1] or [4] is used for manufacturing a semiconductor device in which a semiconductor chip is bonded to another semiconductor chip while burying a part or the whole of a wire connected to the other semiconductor chip. [6]

[0032] The adhesive film for a semiconductor according to any one of [1] to [5], further comprising an elastomer, wherein the content of the elastomer is 10 to 60% by mass based on the mass of the adhesive film. [7]

[0034] The adhesive film for semiconductor according to [6], wherein

[0035] The content of the elastomer is 20 to 55% by mass based on the mass of the adhesive film. [8]

[0037] The adhesive film for a semiconductor according to any one of [1] to [7], further comprising an inorganic filler, wherein the content of the inorganic filler is 60 parts by mass or more based on 100 parts by mass of the thermosetting component. [9]

[0039] The adhesive film for semiconductor according to [8], wherein

[0040] The content of the inorganic filler is 78 to 267 parts by mass based on 100 parts by mass of the thermosetting component.

[10]

[0042] The adhesive film for a semiconductor according to any one of [1] to [9], wherein

[0043] Based on the mass of the adhesive film, the content of the thermosetting component is 15 to 30 mass %.

[11]

[0045] A dicing die bonding film, comprising:

[0046] Cutting film; and

[0047] The adhesive film for a semiconductor according to any one of [1] to

[10] provided on the dicing film.

[12]

[0049] A method for manufacturing a semiconductor device, comprising the step of bonding a second semiconductor chip to a substrate on which a first semiconductor chip is mounted, using the adhesive film described in [1] or [2].

[0050] The first semiconductor chip is embedded through the adhesive film.

[13]

[0052] A method for manufacturing a semiconductor device, comprising the step of bonding a second semiconductor chip to a first semiconductor chip via the adhesive film for a semiconductor according to [1] or [4].

[0053] A wire is connected to the first semiconductor chip,

[0054] A part or the whole of the lead wire is buried through the adhesive film.

[14]

[0056] The method according to

[12] , wherein:

[0057] The first semiconductor chip is a controller chip.

[15]

[0059] The method according to

[13] , wherein:

[0060] The first semiconductor chip is a controller chip.

[0061] Effects of the Invention

[0062] It is possible to improve embedding properties in FOD or FOW while suppressing seepage. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Figure 1 It is a schematic cross-sectional view showing an example of an adhesive film.

[0064] Figure 2 This is a schematic cross-sectional view showing an example of a laminated sheet having an adhesive film.

[0065] Figure 3 This is a schematic cross-sectional view showing an example of a laminated sheet having an adhesive film.

[0066] Figure 4 It is a schematic cross-sectional view showing an example of a semiconductor device.

[0067] Figure 5 This is a process diagram showing an example of a method for manufacturing a semiconductor device.

[0068] Figure 6 This is a process diagram showing an example of a method for manufacturing a semiconductor device.

[0069] Figure 7This is a process diagram showing an example of a method for manufacturing a semiconductor device.

[0070] Figure 8 This is a process diagram showing an example of a method for manufacturing a semiconductor device.

[0071] Fig. 9 This is a process diagram showing an example of a method for manufacturing a semiconductor device.

[0072] Fig.10 is a schematic cross-sectional view showing another example of a semiconductor device.

[0073] Fig.11 is a schematic cross-sectional view showing another example of a semiconductor device. DETAILED DESCRIPTION

[0074] The present invention is not limited to the following examples. In the following examples, except for the cases specifically indicated, the constituent elements (including steps, etc.) are not essential. The sizes of the constituent elements in each figure are conceptual sizes, and the relative relationship between the sizes of the constituent elements is not limited to the relationship shown in each figure. The numerical values ​​and their ranges exemplified below do not limit the present invention either.

[0075] In this specification, the numerical range represented by "~" indicates a range including the numerical values ​​recorded before and after "~" as the minimum value and the maximum value, respectively. In the numerical range recorded in stages in this specification, the upper limit value or lower limit value recorded in one numerical range can also be replaced by the upper limit value or lower limit value of other numerical ranges recorded in stages. In the numerical range recorded in this specification, the upper limit value or lower limit value of the numerical range can be replaced by the value shown in the embodiment.

[0076] In this specification, (meth)acrylate refers to acrylate or its corresponding methacrylate. This also applies to other similar expressions such as (meth)acryloyl, (meth)acrylic acid copolymer, etc.

[0077] Figure 1 It is a schematic cross-sectional view showing an example of an adhesive film. Figure 1 The adhesive film 10 shown may be, for example, a film formed of a thermosetting adhesive containing a thermosetting component, an elastomer, and an inorganic filler. The adhesive film 10 may be in a semi-cured (B-stage) state.

[0078] According to the knowledge of the present inventors, the shear viscosity of the adhesive film 10 in the range of 60 to 150° C., especially at a frequency of 4.4 Hz, is related to the embedding property and the degree of seepage of the adhesive film 10. When the shear viscosity of the adhesive film 10 in the range of 60 to 150° C. at a frequency of 4.4 Hz is at least 2000 Pa·s and at most 200000 Pa·s, the embedding property in the FOD or FOW can be improved while suppressing the seepage.

[0079] From the viewpoint of suppressing bleeding, the minimum value of the shear viscosity at a frequency of 4.4 Hz shown by the adhesive film 10 at 60 to 150° C. may be 2200 Pa·s or more, 2300 Pa·s or more, or 2400 Pa·s or more. The minimum value of the shear viscosity at a frequency of 4.4 Hz shown by the adhesive film 10 at 60 to 150° C. may be 10000 Pa·s or less, 9000 Pa·s or less, 8000 Pa·s or less, or 7000 Pa·s or less.

[0080] From the viewpoint of further improving embedding properties, at 60 to 150° C., the maximum value of the shear viscosity at a frequency of 4.4 Hz shown in the adhesive film 10 may be 180,000 Pa·s or less, 175,000 Pa·s or less, 170,000 Pa·s or less, or 165,000 Pa·s or less. At 60 to 150° C., the maximum value of the shear viscosity at a frequency of 4.4 Hz shown in the adhesive film 10 may be 10,000 Pa·s or more, 11,000 Pa·s or more, 12,000 Pa·s or more, 13,000 Pa·s or more, 14,000 Pa·s or more, 15,000 Pa·s or more, 16,000 Pa·s or more, or 17,000 Pa·s or more.

[0081] The thickness of the adhesive film 10 may be, for example, 1 μm or more, 3 μm or more, 20 μm or more, 30 μm or more, 35 μm or more, 40 μm or more, 50 μm or more, or 60 μm or more, and may be 200 μm or less, 150 μm or less, 120 μm or less, 80 μm or less, or 60 μm or less. When the adhesive film 10 is an adhesive film for FOW, in order to embed the wire so that the wire does not contact the semiconductor chip, the thickness may be, for example, 20 to 120 μm, 25 to 80 μm, or 30 to 60 μm. When the adhesive film 10 is an adhesive film for FOD, in order to appropriately embed the entire semiconductor chip (for example, a controller chip), the thickness of the adhesive film 10 may also be, for example, 40 to 200 μm, 50 to 150 μm, or 80 to 120 μm.

[0082] (a) Thermosetting components

[0083] The thermosetting component contains (a1) a thermosetting resin, which is a compound having a functional group that forms a cross-linked structure by a thermosetting reaction. The thermosetting component may also contain (a2) a curing agent that reacts with the thermosetting resin. From the viewpoint of adhesion, the thermosetting resin may contain an epoxy resin as a compound having an epoxy group. In this case, the curing agent may contain a phenolic resin as a compound having a phenolic hydroxyl group.

[0084] Based on the mass of the adhesive film 10, the content of the thermosetting component (the total content of the thermosetting resin and the curing agent) can be 8% by mass or more, 10% by mass or more, or 15% by mass or more, and can be 80% by mass or less, 70% by mass or less, 60% by mass or less, 50% by mass or less, 45% by mass or less, or 30% by mass or less. When the content of the thermosetting component is high, the adhesive force of the adhesive film after curing tends to be improved. When the content of the thermosetting component is 80% by mass or less, it can be expected that the film-forming property when applying the varnish for forming the adhesive film is ensured.

[0085] Examples of epoxy resins include bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol S epoxy resins, phenol novolac epoxy resins, cresol novolac epoxy resins, bisphenol A novolac epoxy resins, bisphenol F novolac epoxy resins, stilbene epoxy resins, epoxy resins containing triazine skeletons, epoxy resins containing fluorene skeletons, trisphenol methane epoxy resins, biphenyl epoxy resins, xylylene epoxy resins, biphenyl aralkyl epoxy resins, naphthalene epoxy resins, and diglycidyl ether compounds derived from polyfunctional phenol compounds or polycyclic aromatic compounds (anthracene, etc.). These may be used alone or in combination of two or more. From the viewpoint of the adhesiveness and flexibility of the adhesive film, the epoxy resin may be a cresol novolac epoxy resin, a bisphenol F epoxy resin, a bisphenol A epoxy resin, or a combination thereof.

[0086] The thermosetting resin may also contain a liquid epoxy resin as a liquid at 25°C. The content of the liquid epoxy resin may be 5 to 15% by mass based on the mass of the adhesive film 10. The thermosetting resin may also contain an epoxy resin having a softening point lower than 30°C. The adhesive film containing these epoxy resins tends to have good flexibility, and the embedding property of the adhesive film for semiconductor chips and wires is further improved. The thermosetting resin may also contain an epoxy resin having a softening point of 50°C or more.

[0087] As examples of phenolic resins used as curing agents, novolac type phenolic resins, allylated bisphenol A, allylated bisphenol F, allylated naphthalene glycol, phenol aralkyl resins and naphthol aralkyl resins can be cited. These can also be used alone or in combination of two or more. The phenolic resin can be a phenol aralkyl resin, a naphthol aralkyl resin or a combination thereof. Novolac type phenolic resins are obtained by condensing or co-condensing phenols (e.g., phenol, cresol, resorcinol, catechol, bisphenol A, bisphenol F, phenylphenol, aminophenol) and / or naphthols (e.g., α-naphthol, β-naphthol, dihydroxynaphthalene) with compounds having aldehyde groups such as formaldehyde under an acidic catalyst. Phenol aralkyl resins and naphthol aralkyl resins are synthesized from phenol novolac, phenol and / or naphthols with dimethoxy-p-xylene or bis(methoxymethyl)biphenyl.

[0088] The hydroxyl equivalent of the phenolic resin may be 70 g / eq or more, or 70 to 300 g / eq. When the hydroxyl equivalent of the phenolic resin is 70 g / eq or more, the storage elastic modulus of the adhesive film tends to be further increased. When the hydroxyl equivalent of the phenolic resin is 300 g / eq or less, the generation of foaming and degassing can be further suppressed.

[0089] When the thermosetting resin contains an epoxy resin and the curing agent contains a phenolic resin, from the perspective of curability, the ratio of the epoxy equivalent of the epoxy resin to the hydroxyl equivalent of the phenolic resin (epoxy equivalent: hydroxyl equivalent) can be 0.30 / 0.70 to 0.70 / 0.30, 0.35 / 0.65 to 0.65 / 0.35, 0.40 / 0.60 to 0.60 / 0.40, or 0.45 / 0.55 to 0.55 / 0.45. When the equivalent ratio is 0.30 / 0.70 or more, there is a tendency to obtain more sufficient curability. When the equivalent ratio is 0.70 / 0.30 or less, it is possible to prevent the viscosity from becoming too high and obtain more sufficient fluidity.

[0090] The softening point of the curing agent may be 50 to 200° C., or 60 to 150° C. A curing agent having a softening point of 200° C. or less tends to have good compatibility with a thermosetting resin.

[0091] (b) Elastomer

[0092] The elastomer may be, for example, a polymer compound having a glass transition temperature (Tg) of 55° C. or less. Examples of the component (b) include acrylic resins, polyester resins, polyamide resins, polyimide resins, silicone resins, butadiene resins, acrylonitrile resins, and modified products thereof.

[0093] Based on the mass of the adhesive film 10, the content of the elastomer can be 10% by mass or more, 11% by mass or more, 12% by mass or more, 13% by mass or more, 14% by mass or more, 15% by mass or more, 16% by mass or more, 17% by mass or more, 18% by mass or more, 19% by mass or more, or 20% by mass or more, and can be 60% by mass or less, 58% by mass or less, 55% by mass or less, or 50% by mass or less. In the case where the adhesive film contains two or more elastomers, their total amount is the content of the elastomer. When the content of the elastomer is 10% by mass or more, the adhesive film has a high viscosity, and it can be expected to improve the operability of the film and suppress exudation. When the content of the elastomer is 60% by mass or less, there is a tendency for the embedding property to be further improved.

[0094] From the viewpoint of fluidity, the elastomer may contain an acrylic resin. Here, an acrylic resin refers to a polymer containing monomer units derived from (meth)acrylate. Based on the total amount of the acrylic resin, the content of the constituent units derived from (meth)acrylate in the acrylic resin may be, for example, 70% by mass or more, 80% by mass or more, or 90% by mass or more. The acrylic resin may contain monomer units derived from (meth)acrylate having crosslinking functional groups such as epoxy, alcoholic or phenolic hydroxyl, and carboxyl. The acrylic resin may be an acrylic rubber, which is a copolymer containing (meth)acrylate and acrylonitrile as monomer units.

[0095] The glass transition temperature (Tg) of the elastomer (e.g., acrylic resin) may be above -50°C, above -30°C, above 0°C, or above 3°C, and may be below 50°C, below 45°C, below 40°C, below 35°C, below 30°C, or below 25°C. When the Tg of the elastomer is low, the adhesive film tends to have good flexibility. The adhesive film with good flexibility is easily cut together with the semiconductor wafer during cutting, thereby effectively suppressing the generation of burrs. The adhesive film with good flexibility is easy to adhere to the semiconductor wafer while fully eliminating pores, and can also suppress the cracking during cutting caused by reduced adhesion. The glass transition temperature (Tg) refers to the value measured using a DSC (thermal differential scanning calorimeter) (e.g., "Thermo Plus 2" manufactured by Rigaku Corporation). By adjusting the type and content of the constituent units constituting the elastomer (in the case of acrylic resin, the constituent units derived from (meth) acrylate), the Tg of the elastomer can be adjusted to the desired range.

[0096] The weight average molecular weight (Mw) of the elastomer (e.g., acrylic resin) may be 100,000 or more, 200,000 or more, or 300,000 or more, and may be 3,000,000 or less, 2,000,000 or less, or 1,000,000 or less. When the Mw of the elastomer is within such a range, the film forming property, the strength, flexibility, and viscosity of the adhesive film can be properly controlled, and the reflow property is excellent, which can improve the embedding property. Mw refers to the value measured by gel permeation chromatography (GPC) and converted using a calibration curve based on standard polystyrene.

[0097] Examples of commercially available acrylic resins include SG-70L, SG-708-6, WS-023EK30, SG-280EK23, HTR-860P-3CSP, HTR-860P-3CSP-30B (all manufactured by Nagase ChemteX Corporation), and H-CT-865 (manufactured by Showa Denko Materials Co., Ltd.).

[0098] (c) Inorganic fillers

[0099] The inorganic filler may be, for example, particles containing at least one inorganic material selected from aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, aluminum borate whisker, boron nitride and silicon dioxide. From the viewpoint of adjusting the melt viscosity, the inorganic filler may contain silicon dioxide.

[0100] From the perspective of fluidity, the average particle size of the inorganic filler can be 0.01 μm or more, or 0.03 μm or more, and can be 1.5 μm or less, 1.0 μm or less, 0.8 μm or less, 0.08 μm or less, or 0.06 μm or less. Two or more inorganic fillers with different average particle sizes can also be combined. Here, the average particle size refers to the particle size with a cumulative frequency of 50% in the particle size distribution obtained by the laser diffraction / scattering method. The average particle size of the inorganic filler can also be obtained by using an adhesive film containing an inorganic filler. In this case, the residue obtained by heating the adhesive film to decompose the resin component is dispersed in a solvent to prepare a dispersion, and the average particle size of the inorganic filler can be obtained based on the particle size distribution obtained by applying the laser diffraction / scattering method.

[0101] The adhesive film may contain (c1) a first inorganic filler and (c2) a second inorganic filler satisfying all of the following conditions: The adhesive film containing the components (c1) and (c2) can improve embedding properties and, after curing, can improve breaking strength.

[0102] The average particle size of the component (c1) is 300 to 1000 nm.

[0103] The average particle size of the component (c2) is 0.05 to 0.70 times the average particle size of the component (c1).

[0104] The total content of the component (c1) and the component (c2) is 30 to 60% by mass based on the total amount of the adhesive film.

[0105] The average particle size of the component (c1) is 300 to 1000 nm, and may be 350 nm or more, 400 nm or more, or 450 nm or more, and may be 900 nm or less, 800 nm or less, 700 nm or less, or 600 nm or less.

[0106] The average particle size of the component (c2) may be less than 300 nm, or may be 250 nm or less, 220 nm or less, or 200 nm or less. The average particle size of the component (c2) may be, for example, 10 nm or more, 50 nm or more, or 100 nm or more.

[0107] In this specification, these average particle sizes related to the components (c1) and (c2) refer to the particle sizes with a cumulative frequency of 50% in the particle size distribution obtained by the laser diffraction / scattering method. The average particle sizes of the components (c1) and (c2) can also be obtained by using an adhesive film containing the components (c1) and (c2). In this case, the residue obtained by decomposing the resin component by heating the adhesive film is dispersed in a solvent to prepare a dispersion, and based on the particle size distribution obtained by applying the laser diffraction / scattering method thereto, the value of the peak in the range of 300 to 1000 nm can be used as the average particle size of the component (c1), and the value of the peak in the range of less than 300 nm can be used as the average particle size of the component (c2).

[0108] The average particle size of the component (c2) is 0.05 to 0.70 times the average particle size of the component (c1). The average particle size of the component (c2) may be 0.10 times or more, 0.20 times or more, or 0.30 times or more, and may be 0.60 times or less, 0.50 times or less, or 0.40 times or less.

[0109] The content of component (c1) may be 5 to 40% by mass, or 6% or more, 8% or more, or 10% or more, and may be 35% or less, 32% or less, or 30% or less, based on the total amount of the adhesive film.

[0110] The content of component (c2) may be 10 to 50% by mass, or may be 15% or more, 18% or more, or 20% or more, and may be 45% or less, 42% or less, or 40% or less, based on the total amount of the adhesive film.

[0111] Based on the total amount of the adhesive film, the total content of components (c1) and (c2) is 30 to 60% by mass, and can be greater than 35% by mass, greater than 40% by mass, or greater than 45% by mass, and can be less than 55% by mass, less than 52% by mass, or less than 50% by mass.

[0112] Based on the total content of components (c1) and (c2), the content of component (c1) may be 10 to 70% by mass, or may be 15% by mass or more, 18% by mass or more, or 20% by mass or more, and may be 65% by mass or less, 62% by mass or less, or 60% by mass or less.

[0113] Based on the total content of components (c1) and (c2), the content of component (c2) can be 30 to 90% by mass, or can be 35% by mass or more, 38% by mass or more, or 40% by mass or more, and can be 85% by mass or less, 82% by mass or less, or 80% by mass or less.

[0114] The content of the inorganic filler can be 60 parts by mass or more, 65 parts by mass or more, 70 parts by mass or more, or 78 parts by mass or more, and can be 300 parts by mass or less, or 267 parts by mass or less, based on the thermosetting component (the total content of the thermosetting resin and the curing agent). When the content of the inorganic filler is large, the shear viscosity of the adhesive film 10 at a frequency of 4.4 Hz tends to increase. When the content of the inorganic filler is 300 parts by mass or less, it is easy to ensure an appropriate content of the elastomer, so there is a tendency to further improve the film-forming property and operability of the film.

[0115] (d) Coupling agent

[0116] The adhesive film 10 may further contain a coupling agent. The coupling agent may also be a silane coupling agent. Examples of silane coupling agents include γ-ureidopropyltriethoxysilane, γ-mercaptopropyltrimethoxysilane, 3-phenylaminopropyltrimethoxysilane, and 3-(2-aminoethyl)aminopropyltrimethoxysilane. These may also be used alone or in combination of two or more.

[0117] (e) Curing accelerator

[0118] The adhesive film 10 may also contain a curing accelerator that promotes the curing reaction of the thermosetting component. Examples of curing accelerators include imidazole and its derivatives, organophosphorus compounds, secondary amines, tertiary amines and quaternary ammonium salts. These may also be used alone or in combination of two or more. From the viewpoint of reactivity, the curing accelerator may be imidazole or its derivatives. Examples of imidazole derivatives include 2-methylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-phenylimidazole and 1-cyanoethyl-2-methylimidazole. These may also be used alone or in combination of two or more.

[0119] The adhesive film 10 may further contain other components as necessary. Examples of other components include pigments, ion scavengers, and antioxidants.

[0120] The adhesive film 10 can be used as, for example, a protective sheet for protecting the back surface of a semiconductor element of a flip-chip semiconductor device or a sealing sheet for sealing between the surface of a semiconductor element of a flip-chip semiconductor device and an adherend.

[0121] The adhesive film 10 can also be Figure 2 or Figure 3 The laminated sheet is supplied in the form of the laminated sheet illustrated in FIG. Figure 2 The laminated sheet 100 shown includes a substrate 20 and an adhesive film 10 disposed on the substrate 20 . Figure 3 The laminate sheet 110 shown further includes a protective film 30 provided on the surface of the adhesive film 10 on the side opposite to the substrate 20 .

[0122] The substrate 20 may be a resin film, and examples thereof include films of polytetrafluoroethylene, polyethylene, polypropylene, polymethylpentene, polyethylene terephthalate, or polyimide. The thickness of the resin film as the substrate 20 may be, for example, 60 to 200 μm or 70 to 170 μm.

[0123] The substrate 20 may be a dicing film. The laminated sheet in which the substrate 20 is a dicing film can be used as a dicing die bonding film. The dicing die bonding film may be in a tape shape.

[0124] As examples of dicing films, resin films such as polytetrafluoroethylene film, polyethylene terephthalate film, polyethylene film, polypropylene film, polymethylpentene film and polyimide film can be cited. As needed, the dicing film can also be a resin film that has been surface treated by primer coating, UV treatment, corona discharge treatment, grinding treatment or etching treatment. The dicing film can have adhesiveness. The dicing film with adhesiveness can be, for example, a resin film imparted with adhesiveness, or a laminate having a resin film and an adhesive layer disposed on one side thereof. The adhesive layer can be formed by a pressure-sensitive or ultraviolet curing adhesive. A pressure-sensitive adhesive is an adhesive that shows constant adhesiveness under short-term pressure. A radiation-curing adhesive is an adhesive having the property of reducing adhesiveness by irradiation with radiation (e.g., ultraviolet rays). The thickness of the adhesive layer can be appropriately set according to the shape and size of the semiconductor device, for example, 1 to 100 μm, 5 to 70 μm, or 10 to 40 μm. From the viewpoint of economic efficiency and film handling properties, the thickness of the substrate 20 as a dicing film may be 60 to 150 μm or 70 to 130 μm.

[0125] The protective film 30 may be the same resin film as the base material 20. The thickness of the protective film 30 may be, for example, 15 to 200 μm or 70 to 170 μm.

[0126] Semiconductor device and method for manufacturing the same

[0127] Figure 4 2 is a schematic cross-sectional view showing an example of a semiconductor device manufactured using an adhesive film. The semiconductor device 200 is mainly composed of a substrate 14, a first semiconductor chip Wa and a second semiconductor chip Waa mounted on the substrate 14, a sealing layer 42 for sealing the second semiconductor chip Waa, and an adhesive film 10 for bonding the second semiconductor chip Waa to the substrate 14. The substrate 14 has an organic substrate 90 and circuit patterns 84 and 94 provided on the organic substrate 90. The first semiconductor chip Wa is bonded to the substrate 14 by an adhesive 41. The first wire 88 is connected to the first semiconductor chip Wa, and the first semiconductor chip Wa is electrically connected to the circuit pattern 84 via the first wire 88. The first semiconductor chip Wa as a whole and the first wire 88 as a whole are buried in the adhesive film 10. The second wire 98 is connected to the second semiconductor chip Waa, and the second semiconductor chip Waa is electrically connected to the circuit pattern 84 via the second wire 98. The second semiconductor chip Waa as a whole and the second wire 98 as a whole are buried in the sealing layer 42.

[0128] Figure 5 , Figure 6 , Figure 7 , Figure 8 and Fig. 9 It means manufacturing Figure 4 A process diagram of an example of a method for producing a semiconductor device 200. Figures 5 to 9The method shown includes the following steps: bonding the first semiconductor chip Wa to the substrate 14 via the adhesive 41; setting the first wire 88 connecting the first semiconductor chip Wa and the substrate 14 (circuit pattern 84); preparing a chip with adhesive having a second semiconductor chip Wbb and an adhesive film 10 attached thereto; pressing the chip with adhesive onto the substrate 14, thereby bonding the second semiconductor chip Waa to the substrate 14 in a manner that the first semiconductor chip Wa and the first wire 88 are buried through the adhesive film 10; setting the second wire 98 connecting the second semiconductor chip Waa and the substrate 14 (circuit pattern 84). Afterwards, by forming a sealing layer 44, a Figure 4 A semiconductor device 200 is shown.

[0129] The thickness of the first semiconductor chip Wa may be 10 to 170 μm. The first semiconductor chip Wa may be a controller chip for driving the semiconductor device 200. The first semiconductor chip Wa may be a flip chip chip. The size of the first semiconductor chip Wa is usually smaller than the size of the second semiconductor chip Waa. The adhesive 41 between the first semiconductor chip Wa and the substrate 14 may be a common semiconductor adhesive.

[0130] The chip with adhesive formed by the second semiconductor chip Waa and the adhesive film 10 can be used, for example, with Figure 2 The laminated sheet 100 (cutting die bonding film) is prepared by a cutting die bonding film of the same structure as the laminated sheet 100 illustrated in the example. In this case, for example, the laminated sheet 100 (cutting die bonding film) is attached to a single surface of the semiconductor wafer in a direction in which its adhesive film 10 contacts the semiconductor wafer. The surface to which the adhesive film 10 is attached can be the circuit surface of the semiconductor wafer, or it can be the back surface on the opposite side. The semiconductor wafer to which the laminated sheet 100 (cutting die bonding film) is attached is divided by cutting to form a single-piece second semiconductor chip Waa. As examples of cutting, there can be cited a method of cutting using a blade of a rotating knife, and a method of cutting the adhesive film 10 together with the semiconductor wafer by laser. It is also possible to reduce the adhesive force of the cutting film by irradiating ultraviolet rays after cutting. The second semiconductor chip Waa is picked up together with the divided adhesive film 10.

[0131] The second semiconductor chip Waa may have a size of 20 mm or less in width. The width (or length of one side) of the second semiconductor chip Waa may be 3 to 15 mm, or 5 to 10 mm.

[0132] The semiconductor wafer used to form the second semiconductor chip Waa may be, for example, a thin semiconductor wafer having a thickness of 10 to 100 μm. In addition to single crystal silicon, the semiconductor wafer may also be a compound semiconductor wafer such as polycrystalline silicon, various ceramics, or gallium arsenide. The second semiconductor chip Waa may also be formed from the same semiconductor wafer.

[0133] like Figure 7 As shown in FIG. 1 , the chip with adhesive formed by the adhesive film 10 and the second semiconductor chip Waa is placed so that the first wire 88 and the first semiconductor chip Waa are covered by the adhesive film 10. Figure 8 As shown, the second semiconductor chip Waa is fixed to the substrate 14 by pressing the second semiconductor chip Waa onto the substrate 14. The heating temperature for pressing can be 50 to 200°C, or 100 to 150°C. If the heating temperature for pressing is high, the adhesive film 3 becomes soft, so there is a tendency for the embedding property to be further improved. The pressing time can be 0.5 to 20 seconds, or 1 to 5 seconds. The pressure for pressing can be 0.01 to 5 MPa, or 0.02 to 2 MPa.

[0134] After the crimping, the structure including the adhesive film 10 may be further heated to cure the adhesive film 10. The temperature and time for this purpose may be appropriately set according to the curing temperature of the adhesive film 10. The temperature may also be changed in stages. The heating temperature may be, for example, 40 to 300° C. or 60 to 200° C. The heating time may be, for example, 30 to 300 minutes.

[0135] like Fig. 9 As shown, the substrate 14 is electrically connected to the second semiconductor chip Waa via the second wire 98. The second wire 98 may be, for example, a gold wire, an aluminum wire, or a copper wire. The heating temperature for connecting the second wire 98 may be in the range of 80 to 250° C. or 80 to 220° C. The heating time for connecting the second wire 98 may be from a few seconds to a few minutes. In order to connect the second wire 98, vibration energy generated by ultrasound and crimping energy generated by applying pressure may also be applied. The type and connection method of the first wire 88 may also be the same as those of the second wire 98.

[0136] After that, a sealing layer 42 is formed by a sealing material to seal the circuit pattern 84, the second wire 98, and the second semiconductor chip Waa. The sealing layer 42 can be formed by a common method using a mold, for example. After the sealing layer 42 is formed, the adhesive film 10 and the sealing layer 42 can be further thermally cured by heating. The heating temperature for this purpose can be, for example, 165 to 185° C., and the heating time can be about 0.5 to 8 hours.

[0137] Fig.10 FIG. 1 is a schematic cross-sectional view showing another example of a semiconductor device manufactured using an adhesive film. Fig.10The semiconductor device 201 shown is mainly composed of a substrate 14, a first semiconductor chip Wa and a second semiconductor chip Waa mounted on the substrate 14, a sealing layer 42 for sealing the first semiconductor chip Wa and the second semiconductor chip Waa, and an adhesive film 10 for bonding the second semiconductor chip Waa to the first semiconductor chip Wa. The substrate 14 has an organic substrate 90, a circuit pattern 84 provided on the organic substrate 90, and a connection terminal 95 provided on the surface of the organic substrate 90 on the side opposite to the circuit pattern 84. The first semiconductor chip Wa is bonded to the substrate 14 by an adhesive 41. The first wire 88 is connected to the first semiconductor chip Wa, and the first semiconductor chip Wa is electrically connected to the circuit pattern 84 via the first wire 88. A portion of the first wire 88 is buried in the adhesive film 10. The second wire 98 is connected to the second semiconductor chip Waa, and the second semiconductor chip Waa is electrically connected to the circuit pattern 84 via the second wire 98.

[0138] Fig.10 The semiconductor device 201 shown can be manufactured by the same method as the method for manufacturing the semiconductor device 200 , which method includes the step of bonding the second semiconductor chip Waa to the first semiconductor chip Wa via the adhesive film 10 .

[0139] Fig.11 FIG. 1 is a schematic cross-sectional view showing another example of a semiconductor device manufactured using an adhesive film. Fig.11 The semiconductor device 202 shown is mainly composed of a substrate 14 (organic substrate 90), a first semiconductor chip Wa and a second semiconductor chip Waa mounted on the substrate 14, a sealing layer 42 for sealing the first semiconductor chip Wa and the second semiconductor chip Waa, and an adhesive film 10 for burying the first semiconductor chip Wa as a whole and bonding the second semiconductor chip Waa to the substrate 14. The first semiconductor chip Wa is a flip chip type chip and is electrically connected to the substrate 14 via a plurality of electrodes 96. An underfill 50 is filled between the first semiconductor chip Wa and the substrate 14.

[0140] Example

[0141] 1. Preparation of adhesive film

[0142] (1) Raw materials

[0143] The following raw materials were prepared.

[0144] (a1) Thermosetting resin (epoxy resin)

[0145] N-500P-10 (trade name, manufactured by DIC Corporation, o-cresol novolac type epoxy resin, epoxy equivalent: 204 g / eq, softening point: 75 to 85°C)

[0146] EXA-830CRP (trade name, manufactured by DIC Corporation, liquid bisphenol F type epoxy resin, epoxy equivalent: 159 g / eq)

[0147] (a2) Curing agent (phenolic resin)

[0148] MEH-7800M (trade name, manufactured by Meiwa Chemical Industry Co., Ltd., phenyl aralkyl type phenolic resin, hydroxyl equivalent: 174 g / eq, softening point: 80°C)

[0149] PSM-4326 (trade name, manufactured by Gunei Chemical Co., Ltd., phenol novolac resin, hydroxyl equivalent: 105 g / eq, softening point: 120°C)

[0150] ·J-DPP-85 (trade name, manufactured by JFE Chemical Corporation, dicyclopentadiene-type phenolic resin, hydroxyl equivalent: 164 to 167 g / eq, softening point: 85 to 89°C)

[0151] (b) Elastomer (acrylic resin)

[0152] Acrylic resin A (HTR-860P-3CSP (trade name), manufactured by Nagase ChemteX Corporation, acrylic resin, weight average molecular weight: 800,000, Tg: 12°C)

[0153] Acrylic resin B (copolymer of butyl acrylate / ethyl acrylate / ethyl methacrylate / glycidyl methacrylate / styrene, weight average molecular weight: 400,000, Tg: 5°C)

[0154] (c) Inorganic fillers

[0155] Silica filler A (SC2050-HLG (trade name), manufactured by Admatechs Co., Ltd., silica filler dispersion, average particle size: 0.50 μm)

[0156] Silica filler B (silica filler dispersion, average particle size: 0.18 μm)

[0157] (d) Curing accelerator

[0158] ·2PZ-CN (trade name, manufactured by SHIKOKU CHEMICALS CORPORATION, 1-cyanoethyl-2-phenylimidazole)

[0159] (2) Preparation of adhesive varnish

[0160] An adhesive varnish of an embodiment or comparative example containing a thermosetting resin, a curing agent, an elastomer, an inorganic filler and a curing accelerator in the mixing ratio (parts by mass) shown in Table 1, Table 2 or Table 3 is prepared. The mixing ratio of the inorganic filler shown in the table is the amount of solid component (silica filler). A mixture containing a thermosetting resin, a curing agent, an inorganic filler and cyclohexanone is stirred. An elastomer is added thereto and the mixture is stirred. Thereafter, a curing accelerator is added and the mixture is stirred until the components become uniform, thereby obtaining adhesive varnishes of embodiments 1 to 11 and comparative examples 1 to 7. Each adhesive varnish is filtered using a 100 mesh filter. Each adhesive varnish after filtration is vacuum defoamed.

[0161] (3) Adhesive film

[0162] As a support film, a polyethylene terephthalate (PET) film with a thickness of 38 μm and subjected to demolding treatment was prepared. Each adhesive varnish was applied to the support film. The coating film was heated at 90°C for 5 minutes and then heated at 140°C for 5 minutes, and dried by heating in two stages to form an adhesive film (thickness 60 μm) in the B stage state on the support film. The two adhesive films obtained were bonded at 70°C to obtain an adhesive film with a thickness of 120 μm.

[0163] 2. Evaluation

[0164] (1) Shear viscosity of adhesive film

[0165] Multiple adhesive films were bonded together at 80°C to form a laminate with a thickness of 1.1±0.1 mm. A measurement sample with a circular surface of 9 mm in diameter was punched out from the laminate. The measurement sample was mounted on a circular aluminum plate fixture of 8 mm in diameter. The shear viscosity of the measurement sample was measured under the following conditions using ARES (manufactured by TA Instruments Japan Inc.). The minimum and maximum values ​​of the shear viscosity in the range of 60 to 150°C were read from the measurement results. For some adhesive films, the shear viscosity was also measured at a frequency of 1.0 Hz.

[0166] Measurement conditions

[0167] Measuring temperature: 35~160℃

[0168] Heating rate: 5℃ / min

[0169] Strain: 5%

[0170] Frequency: 4.4Hz

[0171] Initial load: 10g

[0172] The shear viscosity of the adhesive film of Example 1 at a frequency of 4.4 Hz is 7900 Pa·s at 80°C and 3500 Pa·s (minimum value) at 129°C. The shear viscosity of the adhesive film of Example 2 at a frequency of 4.4 Hz is 6500 Pa·s at 80°C and 2500 Pa·s (minimum value) at 130°C. The measured values ​​of the shear viscosity of other adhesive films are shown in Table 1.

[0173] (2) Seepage and embedding

[0174] Fabrication of semiconductor devices for evaluation

[0175] A dicing die bonding film (HR-5104-10, adhesive layer thickness: 10 μm, adhesive layer thickness: 110 μm, manufactured by Showa Denko Materials co., Ltd.) having an adhesive layer and an adhesive layer is prepared and attached to a semiconductor wafer (diameter: 8 inches, thickness: 40 μm). The semiconductor wafer attached to the dicing die bonding film is cut by cutting using a fully automatic cutting machine DFD-6361 (manufactured by DISCO Corporation) to form a chip (first semiconductor chip) having a size of 1.6 mm × 4.1 mm. Pick up the chip with adhesive formed by the first semiconductor chip and the adhesive layer attached thereto, and use a crimping machine (die bonding machine manufactured by Besi, trade name: Esec 2100sD PPPplus) to crimp the first semiconductor chip onto the organic substrate via the adhesive layer. The crimping conditions are a temperature of 120°C, a pressure of 0.1 MPa, and a crimping time of 1.5 seconds.

[0176] The adhesive film of each adhesive film (thickness 120μm) of the embodiment or comparative example is bonded to the adhesive film for cutting to produce a cutting die bonding film. The cutting die bonding film is attached to a semiconductor wafer (diameter: 8 inches, thickness: 90μm) in a direction in which the adhesive film contacts the semiconductor wafer. The semiconductor wafer attached to the cutting die bonding film is cut by the same cutting as above to form a second semiconductor chip with a size of 6.0mm×12.0mm. The second semiconductor chip and the adhesive film attached thereto are picked up, and the second semiconductor chip is crimped onto the organic substrate under the conditions of a temperature of 120°C, a pressure of 0.1MPa, and a crimping time of 1.5 seconds so that the first semiconductor chip is covered as a whole by the adhesive film. The position of the second semiconductor chip is adjusted so that the center positions of the first semiconductor chip and the second semiconductor chip are consistent when viewed from above. The formed laminated body was heated at 130° C. for 1 hour at a temperature increase of 15° C. / min to cure the adhesive film, thereby obtaining a semiconductor device for evaluation in which the first semiconductor chip was embedded via the adhesive film.

[0177] Evaluation of exudate

[0178] The upper surface of the second semiconductor chip of the evaluation semiconductor device was observed using a microscope (manufactured by KEYENCE CORPORATION, trade name: VHX-5000). The maximum width (μm) of the adhesive film overflowing from the end of the second semiconductor chip was measured starting from the end of the second semiconductor chip. Based on the obtained value, the amount of bleeding was evaluated according to the following criteria.

[0179] A: less than 100 μm

[0180] B: 100μm or more

[0181] Embedment

[0182] The interface between the cured adhesive film and the first semiconductor chip in the semiconductor device for evaluation was observed using an ultrasonic digital imaging device (manufactured by Insight CO., LTD., trade name: IS-350) at 75 MHz in reflection mode to determine the area ratio of voids in the specified interface. Based on the area ratio, the evaluation was performed according to the following criteria.

[0183] A: The area ratio of pores in a predetermined cross section is less than 5%.

[0184] B: The area ratio of voids in the prescribed cross section is 5% or more.

[0185] [Table 1]

[0186]

[0187] [Table 2]

[0188]

[0189] [Table 3]

[0190]

[0191] As shown in Tables 1 to 3, it can be confirmed that by using an adhesive film having a shear viscosity of at least 2000 Pa·s and at most 200000 Pa·s at a frequency of 4.4 Hz at 60 to 150° C., the semiconductor chip in the lower layer can be sufficiently buried by the adhesive film while suppressing the amount of oozing out.

[0192] Explanation of symbols

[0193] 10-adhesive film, 14-substrate, 20-base material (cutting film), 30-protective film, 41-adhesive, 42-sealing layer, 84, 94-circuit pattern, 88-first conductor, 90-organic substrate, 98-second conductor, 100, 110-laminated sheets, 200, 201, 202-semiconductor device, Wa-first semiconductor chip, Waa-second semiconductor chip.

Claims

1. An adhesive film for semiconductor, comprising a thermosetting component, In the range of 60 to 150° C., the shear viscosity at a frequency of 4.4 Hz is shown to be at least 2,000 Pa·s and at most 200,000 Pa·s. 2 . The adhesive film for a semiconductor according to claim 1 , which has a thickness of 50 to 150 μm. 3 . The adhesive film for a semiconductor according to claim 1 , which is used to bond a semiconductor chip to a substrate while embedding another semiconductor chip. The adhesive film for a semiconductor according to claim 1 , which has a thickness of 25 to 80 μm. 5 . The adhesive film for a semiconductor according to claim 1 , which is used to bond a semiconductor chip to another semiconductor chip while burying a part or the whole of a wire connected to the other semiconductor chip. 6 . The adhesive film for a semiconductor according to claim 1 , further comprising an elastomer, wherein the content of the elastomer is 10 to 60% by mass based on the mass of the adhesive film.

7. The adhesive film for a semiconductor according to claim 6, wherein The content of the elastomer is 20 to 55% by mass based on the mass of the adhesive film. 8 . The adhesive film for a semiconductor according to claim 1 , further comprising an inorganic filler, wherein the content of the inorganic filler is 60 parts by mass or more based on 100 parts by mass of the thermosetting component.

9. The adhesive film for a semiconductor according to claim 8, wherein The content of the inorganic filler is 78 to 267 parts by mass based on 100 parts by mass of the thermosetting component.

10. The adhesive film for a semiconductor according to claim 1, wherein Based on the mass of the adhesive film, the content of the thermosetting component is 15 to 30 mass %.

11. A dicing die bonding film comprising: Cutting film; and The adhesive film for a semiconductor according to claim 1 is provided on the dicing film.

12. A method for manufacturing a semiconductor device, comprising the step of bonding a second semiconductor chip to a substrate on which a first semiconductor chip is mounted, using the adhesive film according to claim 1, The first semiconductor chip is embedded through the adhesive film.

13. A method for manufacturing a semiconductor device, comprising the step of bonding a second semiconductor chip to a first semiconductor chip via the adhesive film for a semiconductor according to claim 1, A wire is connected to the first semiconductor chip, A part or the whole of the lead wire is buried through the adhesive film.

14. The method according to claim 12, wherein: The first semiconductor chip is a controller chip.