Semiconductor material and laminated semiconductor material

By using cellulose materials to form double layer and proton tunneling effects, the problems of toxic elements and environmental pollution in existing semiconductor materials are solved, and the semiconductor materials that are environmentally friendly and biosafe are realized, suitable for a variety of electronic devices .

CN118923231APending Publication Date: 2024-11-08TOHOKU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380033320.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-20
Filing Date
2023-02-13
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

There are toxic elements and environmental pollutants in existing semiconductor materials, and organic semiconductor materials may lead to marine pollution when they are abandoned, and there is a lack of alternative materials that are environmentally friendly to the earth.

Method used

Cellulosic materials from wood, plant fibers, animals, algae and microorganisms are used as the main components of semiconductor materials, and semiconductor characteristics are achieved by forming electric double layers and proton tunneling effects to build renewable, low-environmental burden semiconductor materials.

Benefits of technology

Provides an earth-friendly, less biohazardous semiconductor material with high dielectric domain structure and proton tunneling effect, suitable for DC/AC conversion and semiconductor/metal conduction conversion switching elements, and can operate at low temperatures. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118923231A_ABST
    Figure CN118923231A_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a semiconductor material and a laminated semiconductor material that are friendly to the global environment and have little harm to organisms. [Solution] The present invention is characterized by having a fibrous substance having, as a main component, fibers derived from at least one of wood, plant fibers (pulp), animals, algae, microorganisms, and microbial products, and having an N-type negative resistance. Preferably, the fibrous material is composed of a bundle of cellulose nanofibers (CNF), the width of which is 30-50 nm. In addition, it is preferable that the fibrous substance is configured from a substance in which a plurality of hydroxyl groups and a plurality of carbonyl groups are bonded to cellulose.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to semiconductor materials and stacked semiconductor materials. Background Art

[0002] Semiconductors are used in high-voltage power circuits (high voltage) or electronic and electrical equipment circuits (low voltage) by taking advantage of the fact that their conductivity changes significantly due to the introduction of impurities or the influence of heat, light, magnetic fields, voltage, current, radiation, etc. Semiconductors are widely used, especially in various low-voltage components such as diodes, transistors, FETs, SITs, RAMs, ROMs, CCDs, etc., and are indispensable electronic components for electronic devices. In recent years, high-function IT products such as mobile phones or ultra-small storage devices and batteries for electric vehicles have evolved rapidly, and the demand for further small, large-capacity and high-function semiconductors is increasing. Among them, in particular, a semiconductor suitable for a smart grid (next-generation power grid) society is sought, and the smart grid is in line with green innovation (low carbonization) to prevent global warming.

[0003] In the past, inorganic materials and organic materials can be used as semiconductor materials. As semiconductor materials for electronic and electrical equipment circuits in the weak current field, Si or compound semiconductors are mainly used. For example, the inventors of this application have developed a metal / semiconductor transistor made of an amorphous Ni-Nb-Zr-H alloy (for example, refer to non-patent documents 1 to 5, patent document 1). In addition, organic semiconductors are also used as components of organic EL or organic solar cells, which are the main components of televisions or smart phone products (for example, refer to patent document 2).

[0004] Prior art literature

[0005] Non-patent literature

[0006] Non-patent document 1: M. Fukuhara, A. Kawashima, S. Yamaura, and A. Inoue, "Coulomboscillation of a proton in a Ni-Nb-Zr-H glassy alloy with multiple junctions", Appl. Phys., 2007, 90, 203111

[0007] Non-patent document 2: M.Fukuhara and A.Inoue, "Room-temperature Coulomboscillation of a proton dot in Ni-Nb-Zr-H glassy alloys with nanofaradcapacitance", J.Appl.Phys., 2009,105,063715

[0008] Non-patent document 3: M. Fukuhara, H. Yoshida, K. Koyama, A. Inoue, and Y. Miura, "Electronic transport behaviors of Ni-Ngb-Zr-H glassy alloys", J. Appl. Phys., 2010, 107, 033703

[0009] Non-patent document 4: M.Fukuhara, H.Yoshida, and H.Kawarada, "Effect of hydrogenand cluster morphology on the electronic behavior of Ni-Nb-Zr-H glassy alloys with subnanometer-sized icosahedral Zr5Ni5Nb5 clusters", Euro. Phys.J., 2013, D67,40

[0010] Non-patent literature 5: M. Fukuhara and H. Kawarada, “Room-temperature amorphous alloy field-effect transistor exhibiting particle and wave electronic transport”, J. Appl. Phys., 2015, 117, 084302

[0011] Patent Literature

[0012] Patent Document 1: International Publication No. WO2011 / 037003

[0013] Patent Document 2: Japanese Patent Application Publication No. 2019-130524 Summary of the invention

[0014] 1. Technical issues to be resolved

[0015] The semiconductor material consisting of inorganic materials in the past recorded in non-patent literature 1~5 or patent documentation 1 is a synthetic material, and there are mostly problems that harmful materials are more for protecting the earth's environment or for biological survival including human life. Therefore, as the semiconductor material used, it is expected that the toxic elements such as arsenic, lead, cadmium, beryllium, mercury or environmental pollutants such as lithium, chromium, sulphur are not used, and it is a material that is harmless to health. In addition, for the previous organic semiconductor material recorded in patent documentation 2, there is also a material that causes the increase of carbon dioxide or becomes the material of the microplastics that causes marine pollution when abandoned, mostly harmful materials for protecting the earth's environment or biology.

[0016] The present invention has been completed with an eye on such problems, and an object of the present invention is to provide a semiconductor material and a stacked semiconductor material that are friendly to the global environment and have little harm to living things.

[0017] (II) Technical solution

[0018] The inventors of the present application have discovered that by using a substance having semiconductor conductivity such as cellulose fibers or pulp as an aggregate thereof as a solid semiconductor material, the performance of a diode or a transistor can be exhibited. They thus focused on fibrous materials with wood or plant fibers (pulp) as the main components and completed the present invention.

[0019] That is, in order to achieve the above-mentioned purpose, the semiconductor material of the present invention is characterized in that it has a fibrous material with fibers from at least any one of wood, plant fibers (pulp), animals, algae, microorganisms and microbial products as the main component, and has an N-type negative resistance.

[0020] The fibrous material having fibers from at least any one of wood, plant fiber (pulp), animals, algae, microorganisms and microbial products as the main component is not an environmental pollutant, is recyclable, has a small environmental burden during production and disposal, and is harmless or less harmful to the earth's environment and organisms. The semiconductor material of the present invention has a fibrous material having fibers from at least any one of such wood, plant fiber (pulp), animals, algae, microorganisms and microbial products as the main component, which is friendly to the earth's environment and has little harm to organisms.

[0021] Here, "fibrous material having fibers from at least any one of wood, plant fibers (pulp), animals, algae, microorganisms and microbial products as the main component" means a fibrous material containing fibers using cellulose contained in at least any one of wood, plant fibers (pulp), animals, algae, microorganisms and microbial products as the starting component in the maximum mass proportion.

[0022] The semiconductor material of the present invention is preferably an n-type semiconductor. In this case, the semiconductor material of the present invention is an n-type semiconductor having an N-type negative resistance, which can be used as a DC / AC conversion element or 10 4 Semiconductor / metal conduction conversion switch elements and rectifier circuit elements.

[0023] In the semiconductor material of the present invention, it is preferred that the fiber material is composed of a film, and a double electric layer of electrons and protons can be formed in the film. It is particularly preferred that the fiber material is composed of a material formed by bonding multiple hydroxyl groups and multiple carbonyl groups to cellulose. At this time, a high dielectric domain structure is formed due to the double electric layer formed, and proton tunneling (isolated protons) is formed due to its quantum size effect, thereby expressing semiconductor characteristics. In addition, since a capacitor with countless double electric layers overlapped in a thin film becomes a macroscopic electric lumped constant circuit with limited series connection, it is possible to form a transistor that expresses various functions through dielectric response and direct current. In addition, since the molecular formula (C6H 10 O5) n The polysaccharide cellulose represented by β-glucose is polymerized, so the molecule easily forms hydrogen bonds and becomes sheet-like. It is believed that if the hydroxyl group (OH group) and the carbonyl group (CO group) are bonded to the cellulose, an ordered dipole can be formed in the same direction, which plays the same role as the one-dimensional hydrogen bond chain of water in terms of structure. In other words, it is believed that the movement of the chained proton solitons (Protonic Solitons) can instantly form a double electric layer that is the basis of proton transfer.

[0024] In the semiconductor material of the present invention, the fibrous material can be composed of pulp or cellulose fiber, cellulose nanofiber (CNF), for example. In order to improve the formation efficiency of the double electric layer, it is particularly preferred that the fibrous material is composed of CNF bundles, and the width of the bundle is 30~50nm. In addition, the aspect ratio of the CNF bundle is preferably 1~200, and particularly preferably 1~10. If the aspect ratio of the CNF bundle is greater than 200, the fibers are entangled with each other to form pores, thereby reducing the efficiency. If the aspect ratio is less than 1, the strength is reduced. Since CNF can increase the electron adsorption energy formed by the quantum size effect according to the negative sixth method, when the fibrous material is composed of CNF, the work function can be increased, and the dielectric domain can be further increased, thereby improving the performance as a semiconductor.

[0025] In the semiconductor material of the present invention, when the fiber material is composed of pulp or cellulose fiber, the type of cellulose is not particularly limited. For example, it is possible to use pulp from plants (e.g., wood, bamboo, hemp, jute, kenaf, farmland waste, cloth, pulp (coniferous unbleached kraft pulp (NUKP), coniferous bleached kraft pulp (NBKP), broadleaf unbleached kraft pulp (LUKP), broadleaf bleached kraft pulp (LBKP), coniferous unbleached sulfite pulp (NUSP), coniferous bleached sulfite pulp (NBSP), thermomechanical pulp (TMP), recycled pulp, waste paper) Cellulose from plants or microorganisms is preferred, and cellulose from plants is more preferred. In addition, when the fiber material is composed of CNF, it is preferred that the width of each CNF is about 3 to 4 nm, and it can be an unmodified substance or a chemically modified substance. In addition, the width of CNF is an average fiber diameter, which is an average value of the fiber diameter obtained by observing each fiber using an atomic force microscope (AFM) or a transmission electron microscope (TEM).

[0026] In the semiconductor material of the present invention, the fibrous material is preferably amorphous, but nanocrystals may also be present. In addition, the fibrous material may also have atomic vacancies. In addition, the fibrous material is preferably made of wood or plant fiber (pulp) and is formed by a chemical fiberizing method such as a mechanical fiberizing method or a phosphating method.

[0027] The semiconductor material of the present invention is preferably composed of a bulk semiconductor represented by an equivalent circuit formed by connecting a first RC parallel circuit and a second RC parallel circuit in parallel, wherein the second RC parallel circuit has a resistor greater than the resistance value of the resistor of the first RC parallel circuit and has a capacitor greater than the capacitance of the capacitor of the first RC parallel circuit. In this case, the first RC parallel circuit and the second RC parallel circuit represent a double electric layer in the fiber material, thereby being able to exhibit semiconductor characteristics.

[0028] In addition, at this time, the fiber material is in the form of a thin film sheet, and may also have a pair of metal electrodes respectively arranged on both sides of the fiber material in a manner of clamping the fiber material. At this time, it is equivalent to a lumped constant capacitor having two macroscopic capacitors between each metal electrode. That is, a semiconductor having two bands of a low resistance band for a small current and a high resistance band for a large current can be formed. Each metal electrode can be composed of, for example, Al, Cu, gold, graphite, polyacetylene, polythiophene, etc., and is preferably formed using a microelectromechanical system (M(N)EMS) by sputtering, casting or electrodeposition.

[0029] The semiconductor material of the present invention can be expected to have a lightweight effect, and its thickness is 100 μm or less, preferably a thin film of 5 μm or less. -3 Ωcm or more and 10 8 Ωcm or less, preferably 10 1 Ωcm or more and 10 6 Ωcm or less, preferably 0.1mF / cm 2 More preferably 5mF / cm 2 In addition, the specific surface area of ​​the semiconductor material of the present invention is preferably 800 m 2 In addition, it is preferred that the semiconductor of the present invention can operate at -269°C to 200°C.

[0030] The stacked semiconductor material of the present invention is characterized in that it is composed of a stacked body in which a plurality of semiconductor materials of the present invention are stacked. In this case, for example, the semiconductor material of the present invention can be stacked in series by various M(N)EMS methods, thereby being able to produce a solid quantum semiconductor in which each series equivalent circuit is combined in the form of an electrical lumped constant. In addition, the semiconductor material of the present invention has a pair of metal electrodes, which are composed of a plurality of fiber materials, and can also be composed of a parallel collection body in which each fiber material is arranged along the inner side surface of each metal electrode between each metal electrode. In this case, a withstand voltage of more than 1MV / m can be obtained.

[0031] (III) Beneficial effects

[0032] According to the present invention, it is possible to provide a semiconductor material and a stacked semiconductor material which are friendly to the global environment and have little harm to living things. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 is a circuit diagram showing an equivalent circuit of a semiconductor material according to an embodiment of the present invention.

[0034] Figure 2 is an atomic force microscope (AFM) image of the surface of a mechanically defibrated sheet of semiconductor material as an embodiment of the present invention.

[0035] Figure 3 FIG. 4 is an XRD spectrum of a mechanically defibrated piece of a semiconductor material according to an embodiment of the present invention.

[0036] Figure 4 A graph and a Nyquist plot showing the complex plane of resistance of a mechanically defibrated sheet of semiconductor material as an embodiment of the present invention.

[0037] Figure 5 is a graph showing IV characteristics of a mechanically defibrated sheet of a semiconductor material as an embodiment of the present invention.

[0038] Figure 6 : is a graph showing the results of frequency analysis of the current when a high voltage is applied to a mechanically defibrated sheet of a semiconductor material as an embodiment of the present invention.

[0039] Figure 7 is a graph showing the RV characteristics of a mechanically defibrated sheet of a semiconductor material as an embodiment of the present invention.

[0040] Figure 8 This is a graph showing a complex plane of resistance of a phosphorylated defibrillated sheet of semiconductor material as an embodiment of the present invention.

[0041] Fig. 9 : is a graph showing the IV characteristics of a phosphorylated defibrillated sheet of a semiconductor material as an embodiment of the present invention.

[0042] Fig.10 : is a graph showing the RV characteristics of a phosphorylated defibrillated sheet of a semiconductor material as an embodiment of the present invention.

[0043] Fig.11 This is a graph showing a complex plane of resistance of a chitosan sheet as a semiconductor material according to an embodiment of the present invention.

[0044] Fig.12 : is a graph showing the IV characteristics of a chitosan sheet as a semiconductor material according to an embodiment of the present invention.

[0045] Fig.13 : is a graph showing the frequency analysis result of the current of the chitosan sheet which is the semiconductor material of the embodiment of the present invention in the negative resistance region of the N type.

[0046] Fig.14 (a) to (c) are side views, (d) is a perspective view, and (e) is a side view showing a method for manufacturing a stacked semiconductor material using a MEMS method according to an embodiment of the present invention. DETAILED DESCRIPTION

[0047] The following describes the embodiments of the present invention based on the accompanying drawings and examples.

[0048] Figure 1 to Figure 13 Semiconductor materials according to embodiments of the present invention are shown.

[0049] The semiconductor material of the embodiment of the present invention is composed of a bulk semiconductor, which has a fiber material having at least one fiber from wood, plant fiber (pulp), animal, algae, microorganism, and microorganism product as a main component. As shown in the following structural formula, the fiber material is composed of a molecular formula (C6H 10 O5)n The fiber structure is composed of hydroxyl groups (OH groups) and carbonyl groups (CO groups) bonded to cellulose, a polysaccharide.

[0050] [Chemical formula 1]

[0051]

[0052] The fibrous material is composed of, for example, pulp, cellulose fiber or cellulose nanofiber (CNF). In addition, the fibrous material is amorphous, but nanocrystals may also be present. In addition, the fibrous material may have atomic vacancies. The fibrous material is made of wood or plant fiber (pulp) and is formed by chemical fiberizing methods such as mechanical fiberizing or phosphoric acid esterification.

[0053] Next, its function will be described.

[0054] The semiconductor material of the embodiment of the present invention is easy to form a film sheet due to the cellulose material having β-glucose polymerized from molecular hydrogen bonding. In addition, since the cellulose is bonded with hydroxyl (OH group) and carbonyl (CO group), a double electric layer as the basis of proton transfer can be formed instantly through the action of chained proton solitons. Since a high dielectric domain structure is formed due to the formed double electric layer, and proton tunneling (isolated protons) is formed due to its quantum size effect, semiconductor properties can be exhibited.

[0055] Figure 1 FIG. 2 shows an equivalent circuit of a semiconductor material according to an embodiment of the present invention. Figure 1 As shown, the semiconductor material of the embodiment of the present invention can be represented by an equivalent circuit formed by connecting a first RC parallel circuit 11 and a second RC parallel circuit 12 in parallel, wherein the second RC parallel circuit 12 has a resistor R2 having a larger resistance value than the resistor R1 of the first RC parallel circuit 11, and has a capacitor C2 having a larger capacitance than the capacitor C1 of the first RC parallel circuit 11. The first RC parallel circuit 11 and the second RC parallel circuit 12 represent a double electric layer in the fiber material, thereby being able to exhibit semiconductor characteristics.

[0056] The semiconductor material according to the embodiment of the present invention has fibers mainly composed of fibers derived from at least any one of wood, plant fibers (pulp), animals, algae, microorganisms, and microbial products, and is environmentally friendly and less harmful to organisms.

[0057] The following examples are provided for the purpose of describing the present invention and are not intended to define or restrict the scope of the invention disclosed in this application.

[0058] Example 1

[0059] <Sample 1>

[0060] The semiconductor material of the embodiment of the present invention of Sample 1 was produced in the following manner.

[0061] The stems of kenaf produced in Bangladesh were used as raw materials. After drying and storing, the stems of kenaf were soaked in water at 20°C for two weeks. After two weeks, the white bark on the surface was peeled off and dried. After drying, the fiber was defibrated by a high-pressure homogenizer to make pulped fibers (bast fibers). The sheet pulp was made into a concentration of 3% and soaked in distilled water for 5 hours, and dissociated using a paddle mill for 30 minutes. The dissociated pulp was crushed for 10 hours using a planetary ball mill and zirconia balls at a speed of 100 rpm. The crushed 2% dissociated pulp was dripped onto the Si substrate of the spin coater and rotated at 500 rpm to make a film. Then, the water was evaporated using a heating plate at 100°C to make kenaf sheets.

[0062] The surface of the sheet-like sample 1 was observed using an atomic force microscope (AFM). The results are shown in FIG. Figure 2 .like Figure 2 As shown, it can be confirmed that a plurality of elongated substances with a width of 30 to 50 nm are distributed on the surface of sample 1. Since each CNF has a width of 3 to 4 nm, these substances are considered to be CNF bundles.

[0063] Sample 1 was analyzed by X-ray diffraction (XRD). The obtained XRD spectrum is shown in FIG. Figure 3 .like Figure 3 As shown, since a relatively broad spectrum peak was confirmed, it was confirmed that Sample 1 was amorphous.

[0064] In addition, the density of sample 1 was measured and found to be 1.6 g / cm 3 It was confirmed that the specific gravity was low, less than 2. In addition, it was confirmed that Sample 1 could be operated in a low-medium temperature furnace within the range of -269°C to 200°C up to 300V. In addition, the specific surface area of ​​Sample 1 was measured by the BET method and the result was 800m 2 / g.

[0065] A pair of metal electrodes are set on both sides of a thin film sheet sample 1 so as to sandwich the sample 1, and various measurements are performed. First, an AC signal is applied between the electrodes by the AC resistance method to measure the absolute value of the resistance of the sample 1 and the phase difference between the voltage and the current. In addition, both electrodes are Al electrodes. The measurement results are plotted on a complex plane and are shown in the figure. Figure 4 .like Figure 4As shown in FIG. 1 , it can be confirmed that the measurement result is drawn along the shape of two large and small arcs in parallel. Based on this result, it can be considered that sample 1 can be made Figure 1 The equivalent circuit shown is used to represent it.

[0066] Therefore, in Figure 1 In the equivalent circuit shown in the figure, the resistivity of resistors R1 and R2 and the capacitance of capacitors C1 and C2 are changed, and the least square method is used to find the best fit. Figure 4 The Nyquist plot of the measurement results is shown in Figure 4 The solid line represents the resistivity and capacitance at this time: R1 = 0.35 kΩm, R2 = 8 kΩm, C1 = 2 × 10 -9 F, C2=5×10 -8 F.

[0067] like Figure 4 As shown in the figure, the measurement results are basically consistent with the Nyquist curve, which can confirm that sample 1 is Figure 1 The lumped constant capacitor with two macroscopic capacitors (double layers) shown is equivalent to a semiconductor with two bands, a low resistance band for small currents and a high resistance band for large currents. Based on this result, it can be considered that sample 1 is a bulk semiconductor phenomenon that does not have a pn junction.

[0068] Next, a voltage was applied between the electrodes of Sample 1, and its IV characteristics at room temperature were measured. The results are shown in Figure 5 .like Figure 5 As shown, it can be confirmed that the current of sample 1 decreases between about 15 and 33 V, showing an N-type negative resistance. Based on this result, it can be considered that sample 1 is a semiconductor.

[0069] In addition, a voltage was applied between the electrodes of Sample 1, and the current flowing between the electrodes was measured and its frequency was analyzed. The results are shown in Figure 6 .like Figure 6 As shown in FIG. 1 , harmonic peaks were confirmed at approximately 1 kHz, 3 kHz, and 5 kHz. Based on this result, it can be considered that sample 1 performed DC / AC conversion. In addition, this result is similar to the Gunn effect confirmed in GaAs (gallium arsenide) semiconductors.

[0070] In addition, a voltage was applied between the electrodes of Sample 1, and the RV characteristics at room temperature were measured. The measurement results are shown in FIG. Figure 7 .like Figure 7As shown, it can be confirmed that the resistance value of sample 1 can rise rapidly by about 3 to 4 digits between 0V and about 2V as the voltage rises, and then decreases by about 3 digits. It can be considered that this result is caused by the switching effect between metal and insulator. This is because it is not the effect of a pn-junction semiconductor, but the effect of a semiconductor having two bands, a small current low resistance band and a large current high resistance band, which are unique to an n-type bulk semiconductor with an N-type negative resistance.

[0071] Example 2

[0072] <Sample 2>

[0073] The semiconductor material of the embodiment of the present invention of Sample 2 was produced in the following manner.

[0074] As a raw material, bleached unbeaten kraft pulp (whiteness 85%) from coniferous trees was used, and 10 g of the pulp was immersed in a mixture of urea (12 g) and NH4H2PO4 (4.5 g) added to distilled water (15 g). The impregnated pulp was removed from the mixture and dried, and then cured at 165°C for 10 minutes. The cured pulp was added to distilled water to make a 2% aqueous solution, and caustic soda was further added to neutralize it while maintaining pH 12. The aqueous solution was defibrated using a high-pressure homogenizer to prepare a dispersion of cellulose fibers with a diameter of 30 to 10 nm. The slurry dispersion (2% concentration) was sheeted using a 50°C heated scraper (Doctor Blade) by a scraper method.

[0075] The density of sample 2 was measured and the result was 1.5 g / cm 3 It was confirmed that the specific gravity was low, being less than 2. In addition, it was confirmed that Sample 2 could be operated in a low-medium temperature furnace within a range of -269°C to 200°C up to 300V. In addition, the specific surface area of ​​Sample 2 was measured by the BET method, and the result was 750m 2 / g.

[0076] A pair of metal electrodes are placed on both sides of a thin film sheet sample 2 so as to sandwich the sample 2, and various measurements are performed. First, an AC signal is applied between the electrodes by the AC resistance method to measure the absolute value of the resistance of the sample 2 and the phase difference between the voltage and the current. In addition, one of the electrodes is an Al electrode and the other is a Cu electrode. The measurement results are plotted on a plurality of planes and are shown in FIG. Figure 8 .like Figure 8 As shown in FIG. 1 , it can be confirmed that the measurement results are a graph formed along the shape of two large and small arcs arranged in parallel. Based on these results, it can be considered that sample 2 can be made of Figure 1 The equivalent circuit shown is used to represent it.

[0077] Therefore, in Figure 1In the equivalent circuit shown in the figure, the resistivity of resistors R1 and R2 and the capacitance of capacitors C1 and C2 are changed, and the least square method is used to find the best fit. Figure 8 The Quest curve of the measurement results is shown in Figure 1. The resistivity and capacitance at this time are R1 = 1.4 kΩm, R2 = 5.7 kΩm, C1 = 1.4×10 -6 F, C2 = 2.4 × 10 -5 F.

[0078] The measured results are basically consistent with the Nyquist curve. Figure 1 As shown, sample 2 is equivalent to a lumped constant capacitor with two macroscopic capacitors (double electric layers), and it can be confirmed that a semiconductor with two bands of low resistance band for small current and high resistance band for large current is formed. Based on the results, it can be considered that sample 1 is a non-pn junction and exhibits a bulk semiconductor phenomenon.

[0079] Next, a voltage was applied between the electrodes of Sample 2, and the IV characteristics at room temperature were measured. The results are shown in Fig. 9 .like Fig. 9 As shown, the current of sample 2 decreases between about -150 and -125 V, showing negative resistance of N type. Based on this result, it can be said that sample 2 is a semiconductor.

[0080] In addition, a voltage was applied between the electrodes of Sample 2, and the RV characteristics at room temperature were measured. The measurement results are shown in FIG. Fig.10 .like Fig.10 As shown in the figure, it can be confirmed that the resistance value of sample 2 rises rapidly by about 3 to 4 digits from 0V to about -2.5V as the voltage decreases, and then decreases by about 3 digits. It can be considered that this result is caused by the switching effect between metal and insulator. It can be considered that this is not the effect of the semiconductor of the pn junction, but the effect of the semiconductor having two bands, a small current low resistance band and a large current high resistance band, which are unique to the n-type bulk semiconductor with N-type negative resistance.

[0081] Example 3

[0082] <Sample 3>

[0083] The semiconductor material of the embodiment of the present invention of Sample 3 was produced in the following manner.

[0084] Chitosan was isolated from the shell of red snow crab as raw material. 10 g of chitosan was added to 48% sodium hydroxide solution, boiled at 120°C for 30 minutes, filtered, and completely washed with water to remove sodium hydroxide. The filtered slurry was crushed for 20 hours using a planetary ball mill and zirconia balls at 200 rpm. 3% of the crushed slurry was added dropwise to the Si substrate of a spin coater and rotated at 800 rpm to make it into a thin film. Then, the water was evaporated on a hot plate at 100°C to make chitosan sheets.

[0085] The density of sample 3 was measured and the result was 2.1 g / cm 3 It was confirmed that the specific gravity was relatively low. In addition, it was confirmed that Sample 3 could be operated in a low-medium temperature furnace within the range of -50°C to 200°C up to 300V.

[0086] A pair of metal electrodes were placed on both sides of a thin film sheet sample 3 so as to sandwich the sample 3, and various measurements were performed. First, an AC signal was applied between the electrodes by the AC resistance method, and the absolute value of the resistance of the sample 3 and the phase difference between the voltage and the current were measured. In addition, one of the electrodes was an Al electrode and the other was a Cu electrode. The measurement results were plotted on a plurality of planes and are shown in FIG. Fig.11 .like Fig.11 As shown in FIG. 1 , it can be confirmed that the measurement result is a graph made along the shape of two roughly large and small arcs arranged in parallel. Based on this result, it can be considered that sample 3 can be made Figure 1 The equivalent circuit shown is used to represent it.

[0087] Therefore, in Figure 1 In the equivalent circuit shown in the figure, the resistivity of resistors R1 and R2 and the capacitance of capacitors C1 and C2 are changed, and the least square method is used to find the best fit. Fig.11 The Nyquist plot of the measurement results is shown in Figure 1. The resistivity and capacitance at this time are R1=R2=3.8kΩm, C1=3.3×10 -7 F, C2 = 9.3 × 10 -7 F.

[0088] According to the measurement results, which are basically consistent with the Nyquist curve, sample 3 and Figure 1 The lumped constant capacitor equivalent with two macroscopic capacitors (double electric layers) shown above can confirm the formation of a semiconductor with two bands: a low-resistance band with a small current and a high-resistance band with a large current. Based on this result, it can be considered that sample 3 is a non-pn junction and exhibits a bulk semiconductor phenomenon.

[0089] Next, a voltage was applied between the electrodes of sample 3 to measure the IV characteristics at room temperature. In the measurement, the voltage was applied while scanning from about -210 V to about +30 V at a rate of 1.24 V / s. The results are shown in Fig.12 .like Fig.12 As shown, the current value of sample 3 oscillates between about -210V and about -170V, and it can be confirmed that it exhibits an N-type negative resistance. In addition, since it falls into the 100kΩ resistance region between -170V and 0V, the current is zero, but if it exceeds 0V and enters the positive voltage region, the current flows rapidly, and it can be confirmed that a rectification effect is exhibited.

[0090] Next, the frequency analysis of the current vibration between about -210V and about -170V in the N-type negative resistance region was performed using an oscilloscope. The results are shown in Fig.13 .like Fig.13 As shown in FIG. 1 , a spectrum peak was confirmed at a position where the average frequency was about 40 MHz. Based on this result, it can be considered that sample 3 performed DC / AC conversion.

[0091] Table 1 summarizes the defibration treatment methods, fiber material states (crystal and amorphous), density, resistivity, and capacitance of Samples 1 to 3.

[0092] [Table 1]

[0093]

[0094] Fig.14 A stacked semiconductor material according to an embodiment of the present invention is shown.

[0095] like Fig.14 As shown in FIG. 1 , the laminated semiconductor material of the embodiment of the present invention is manufactured by the MEMS method using the sheet-shaped semiconductor material of the embodiment of the present invention in the following manner. First, as Fig.14 As shown in (a), a Cu layer (500 nm thick) 22 is formed on the surface of a glass substrate (40×40×0.5 mm) 21 by sputtering. Fig.14 As shown in (b), a sheet-shaped semiconductor material 10 is supported on the Cu layer 22, and further, as shown in Fig.14 As shown in (c), an Al layer (500 nm thick) 23 is formed thereon by sputtering. Thus, it is possible to manufacture Fig.14 The material shown in (d) has a Cu layer 22 and an Al layer 23 as metal electrodes on both sides of a sheet-like semiconductor material 10. This structure corresponds to the material having metal electrodes on both sides of samples 1 to 3 used in various measurements of Examples 1 to 3.

[0096] Next, the glass substrate 21 is removed and used as a basic body. By stacking a plurality of these basic bodies, a Fig.14(e) shows a stacked semiconductor material 20 according to an embodiment of the present invention. The stacked semiconductor material 20 is manufactured by connecting a plurality of semiconductor materials 10 in series using the Al layer 23 of the uppermost base body and the Cu layer 22 of the lowermost base body as terminals.

[0097] In this way, the stacked semiconductor material 20 according to the embodiment of the present invention can be composed of a stacked body of a plurality of semiconductor materials 10 according to the embodiment of the present invention, and can be made into a solid quantum semiconductor in which each parallel equivalent circuit is connected in the form of an electrical lumped constant.

[0098] Industrial Applicability

[0099] The semiconductor material and stacked semiconductor material of the present invention can be widely used in weak current fields such as mobile phones, drones, wall-mounted TVs, and strong current fields such as not only automobiles but also ships and airplanes. More specifically, for example, it can be used in AC transmitters or control equipment of microelectronic circuits, overcurrent protection switches, etc. In addition, it can also be used for power modules such as lightning arresters, welding, over-discharge protection, or various amplifiers, microwave transmitters, pump sources for parametric amplifiers, police radars, door opening and closing systems, illegal intrusion detection systems, noise filters, pedestrian safety systems, etc. Sensors, microelectronic control equipment, long-distance vibration detectors, shunt regulators, protection circuits or transmitters, etc. Electronic and electrical substrates, etc.

[0100] Description of Reference Numerals

[0101] 10: semiconductor material; 11: first RC parallel circuit; 12: second RC parallel circuit; 20: stacked semiconductor material; 21: glass substrate; 22: Cu layer; 23: Al layer.

Claims

1. A semiconductor material, characterized in that: The semiconductor material has a fiber material having as a main component fibers derived from at least any one of wood, plant fiber (pulp), animals, algae, microorganisms, and microorganism products, and has an N-type negative resistance.

2. The semiconductor material according to claim 1, characterized in that The semiconductor material is an n-type semiconductor.

3. The semiconductor material according to claim 1 or 2, characterized in that: The fiber material is composed of cellulose nanofiber (CNF) bundles, and the width of the bundles is 30-50 nm.

4. The semiconductor material according to claim 1 or 2, characterized in that: The fiber material is composed of cellulose nanofiber (CNF) bundles, and the aspect ratio of the bundles is 1-200.

5. The semiconductor material according to claim 1 or 2, characterized in that: The fiber material is composed of cellulose to which a plurality of hydroxyl groups and a plurality of carbonyl groups are bonded.

6. The semiconductor material according to claim 1 or 2, characterized in that: The semiconductor material is composed of a bulk semiconductor represented by an equivalent circuit formed by connecting a first RC parallel circuit and a second RC parallel circuit in parallel, The second RC parallel circuit has a resistance greater than a resistance value of a resistance of the first RC parallel circuit, and has a capacitor greater than a capacitance of a capacitor of the first RC parallel circuit.

7. The semiconductor material according to claim 1 or 2, characterized in that: The fibrous material is amorphous.

8. A stacked semiconductor material, characterized in that: The semiconductor material according to claim 1 or 2 is formed by laminating a plurality of semiconductor materials.