Fibrous ring repairing double-layer hydrogel stent embedded with 3D silk fibers and preparation method of fibrous ring repairing double-layer hydrogel stent

By designing a double-layer hydrogel scaffold embedded in 3D silk fibers, the problems of insufficient mechanical strength and weak cell differentiation ability in fibre annulus repair are solved, and physiological repair and regeneration of fibre annulus are achieved, which reduces the risk of postoperative recurrence and provides Good biocompatibility and mechanical properties.

CN118924945APending Publication Date: 2024-11-12SHANGHAI JIAOTONG UNIV +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410926963.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing annular fibrosal repair technology cannot effectively restore the physiological function and mechanical characteristics of the intervertebral disc, resulting in recurrence of annular fibrosal injury and degeneration of the nucleus pulposus. Insufficient mechanical strength of the hydrogel stent leads to insufficient bonding with the annular fibrosal.

Method used

Design a double-layer hydrogel scaffold embedded in 3D silk fibers, including a high-density PEG hydrogel layer and a low-density PEG hydrogel layer. The low-density layer is embedded in the 3D silk fiber structure, by adjusting the number of polyethylene glycol arms and Cross-linking method improves the mechanical strength and biodegradability of the scaffold and promotes stem cell differentiation by loading cytokines.

Benefits of technology

Effective repair and regeneration of the fibroin ring is achieved, the adhesion and mechanical strength of the scaffold are improved, the probability of postoperative recurrence is reduced, the favorable cell differentiation environment is provided, and the biocompatibility and mechanical properties of the fibroin ring are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118924945A_ABST
    Figure CN118924945A_ABST
Patent Text Reader

Abstract

The invention relates to the field of fibrous ring repair and regeneration, in particular to a fibrous ring repair double-layer hydrogel stent embedded with 3D silk fibers and a preparation method of the fibrous ring repair double-layer hydrogel stent. The 3D silk fiber hydrogel comprises an HD-PEG hydrogel layer and an LD-PEG hydrogel layer from top to bottom, a 3D silk fiber structure is embedded in the LD-PEG hydrogel layer, the HD-PEG hydrogel layer is made of 8-arm polyethylene glycol-norbornene, and the LD-PEG hydrogel layer is made of 4-arm polyethylene glycol-norbornene. Compared with the prior art, the obtained double-layer hydrogel scaffold has good adhesion, biocompatibility and mechanical strength, meanwhile, by loading different cell factors, directional differentiation of bone marrow mesenchymal stem cells to fibrous ring inner-layer cartilage-like cells and outer-layer fibroblasts is facilitated, a favorable place is provided for cell differentiation, and the scaffold has good application prospects. The problem that in fibrous ring tissue engineering repair, the differentiation repair capacity of seed stem cells in a hydrogel scaffold is weakened due to the influence of a microenvironment is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of annulus fibrosus repair and regeneration, and specifically to annulus fibrosus repair double-layer hydrogel scaffold embedded with 3D silk fibers and a preparation method thereof. The invention realizes physiological repair of annulus fibrosus by regulating the directional differentiation of bone marrow mesenchymal stem cells (BMSC) in the scaffold into chondrocytes in the inner layer and fibroblasts in the outer layer of the annulus fibrosus, and is suitable for tissue repair and reconstruction surgery. Background Art

[0002] Lumbar disc herniation compressing nerve roots can lead to limb numbness, pain, weakened muscle strength, and even cauda equina syndrome and incomplete paralysis, which not only affects work and quality of life, but also affects society and family. Surgery for disc herniation is currently a common radical treatment, but even with the most minimally invasive fully endoscopic disc herniation, there is still about 5-15% recurrence of disc herniation or lumbar instability after surgery, which troubles both doctors and patients.

[0003] The main causes of these problems are damage to the annulus fibrosus during surgery or poor healing of the original rupture. Even if the annulus fibrosus can be sutured to close the rupture during surgery, this physical form of closure is still insufficient to restore the physiological function of the annulus fibrosus. Injury to the annulus fibrosus not only breaks the immune isolation effect of the nucleus pulposus, thereby aggravating the inflammatory response and degeneration of the intervertebral disc, but is also the main cause of postoperative nucleus pulposus re-herniation [Fu Yu et al., Chinese Journal of Orthopedics, 2023, 31(20): 1870-1874].

[0004] Therefore, in-depth research and exploration of methods for repairing the annulus fibrosus is crucial to improve the efficacy of nucleus pulposus removal, avoid recurrence of herniation, and delay nucleus pulposus degeneration. At present, the means of repairing annulus fibrosus defects include direct suture repair technology and tissue engineering scaffold repair technology. The former can complete the physical occlusion of the annulus fibrosus and prevent the re-herniation of the nucleus pulposus, but it cannot restore the internal structure and mechanical characteristics of the annulus fibrosus of the intervertebral disc, let alone promote the regeneration of the intervertebral disc, and it is difficult to meet the needs of biological repair. Tissue engineering technology has developed rapidly in recent years and has achieved good results in the biological repair of various tissues. Therefore, it has been introduced into the field of annulus fibrosus repair and has made certain progress. Many studies have shown that current biomaterials can effectively fill annulus fibrosus defects. However, in addition to meeting the general characteristics of good biocompatibility, non-toxicity to cells and humans, and degradability, the tissue engineering scaffold for annulus fibrosus repair must also meet the unique biomechanical characteristics of the annulus fibrosus, such as anisotropy, nonlinearity, and viscoelasticity [Ning Qing et al., Chinese Journal of Spine and Spinal Cord, 2023, 33(08):753-759].

[0005] The three-dimensional structure of the annulus fibrosus is complex and varied. The whole is composed of multiple concentric circular plates arranged coaxially. The fibers in the same layer are arranged in parallel, while the fibers in adjacent layers are interwoven at a certain angle. There is a large amount of extracellular matrix between the layers and the fibers. Therefore, the complex multi-layer structure of the annulus fibrosus leads to poor adhesion between the annulus fibrosus stump and the filled tissue engineering materials after degeneration and injury. In addition, the irregular stump morphology further hinders the interface bonding between hard tissue engineering scaffolds such as electrospinning and the annulus fibrosus stump [Tang G#, Frontiers in Bioengineering and Biotechnology, 2020, 8(1084).].

[0006] As an emerging biomaterial in the field of intervertebral disc repair in recent years, hydrogels have three-dimensional cross-linked network structures, adjustable physical and chemical properties, and extracellular matrix-like characteristics, which can be used for cell adhesion and proliferation [5-6]. The design concept of hydrogels integrates the structural integrity, biocompatibility, biodegradability, safety, solute transport, mechanical strength and viscosity of the implant. By selecting different hydrogel component types, cross-linking methods, and modification methods, hydrogels exhibit multiple composite functions as filling implants. However, many hydrogels do not meet the mechanical properties required for articular cartilage repair. Therefore, multilayer hydrogels with different mechanical properties have been proposed as candidate biomaterials for articular cartilage repair. In recent years, research on double-layer hydrogels as scaffolds for annular fibrous repair has become increasingly in-depth. Summary of the invention

[0007] In order to overcome the deficiencies of the prior art, the present invention provides a double-layer hydrogel scaffold for repairing annulus fibrosus embedded with 3D silk fibers and a preparation method thereof. The addition of silk fibers can improve the mechanical strength of the hydrogel to solve the problem that the strength of the hydrogel scaffold is insufficient when repairing the annulus fibrosus, thereby causing the annulus fibrosus and the hydrogel scaffold to be not tightly bonded. At the same time, the hydrogel has good biodegradability, stem cell encapsulation and the ability to promote the differentiation of stem cells into chondrocytes, which is conducive to the successful tissue engineering repair of the annulus fibrosus and reduces the probability of recurrence after lumbar disc herniation surgery.

[0008] To achieve the above objectives, a double-layer hydrogel scaffold for annular fiber repair embedded with 3D silk fibers was designed, which included a HD-PEG hydrogel layer and a LD-PEG hydrogel layer from top to bottom. A 3D silk fiber structure was embedded in the LD-PEG hydrogel layer. The material of the HD-PEG hydrogel layer was 8-arm polyethylene glycol-norbornene, and the material of the LD-PEG hydrogel layer was 4-arm polyethylene glycol-norbornene.

[0009] The 3D silk fiber structure comprises several layers of silk fiber structures, each layer of silk fiber structure is distributed in an S shape or a grid shape; the material of the 3D silk fiber structure is selected from one or more of natural silk, polylactic acid PLA, and polycaprolactone PCL.

[0010] To achieve the above purpose, a method for preparing a double-layer hydrogel scaffold for repairing annulus fibrosus embedded with 3D silk fibers is designed, comprising the following steps: S1, prepare HD-PEG hydrogel and LD-PEG hydrogel respectively; S2, preparing a 3D silk fiber structure: S21, pasting a number of ball steel pins on the PDMS mold according to a predetermined pattern to form a pile frame; S22, moving silk fibers around each pile to form a layer of silk fiber structure; S23, repeating step S22 to obtain a number of layers of silk fiber structure; S24, vertically stacking the several layers of silk fiber structure to form a 3D silk fiber structure; S3, treating the 3D silk fiber structure: S31, applying a silk fibroin solution on the 3D silk fiber structure, and subjecting the 3D silk fiber structure to a vacuum treatment so that the silk fibroin solution completely penetrates into the 3D silk fiber; S32, immersing the 3D silk fiber structure in ethanol to stabilize the structure of the silk fibroin coating, and removing the coating after drying to obtain a treated 3D silk fiber structure; S4, preparing a double-layer hydrogel scaffold: S41, immersing the treated 3D silk fiber structure in an LD-PEG precursor solution, vacuuming to remove air pockets in the 3D silk fiber structure, irradiating under ultraviolet light, swelling to an equilibrium state and then cutting to obtain an LD-PEG hydrogel layer embedded with the 3D silk fiber structure; S42, placing the LD-PEG hydrogel layer obtained in step S41 between two glass sheets, injecting the precursor solution of HD-PEG hydrogel therein, irradiating with ultraviolet light, separating from the glass sheet after photocrosslinking, and swelling to an equilibrium state in PBS to obtain a double-layer hydrogel scaffold.

[0011] The specific method of step S1 is as follows: S11, drying polyethylene glycol in a vacuum, dissolving the dried polyethylene glycol in a mixed solution and stirring at room temperature to obtain a mixture; S12, adding p-nitrophenyl chloroformate dropwise to the above mixture, activating and stirring under a nitrogen atmosphere, precipitating in cold ether and vacuum drying to obtain polyethylene glycol-norbornene.

[0012] In the step S1, the polyethylene glycol selected for the HD-PEG hydrogel includes PEG8OH, and 8-arm polyethylene glycol-norbornene is prepared; the polyethylene glycol selected for the LD-PEG hydrogel includes PEG4OH, and 4-arm polyethylene glycol-norbornene is prepared.

[0013] In the step S11, the mixed solution includes one or more of anhydrous dichloromethane, 4-dimethylaminopyridine, and trimethylamine, and the stirring time is 10-20 minutes to obtain a mixed solution.

[0014] In the step S12, p-nitrophenyl chloroformate is added dropwise to the mixture, and the mixture is stirred continuously at room temperature for 20-28 hours, and polyethylene glycol-norbornene is obtained by cold ether precipitation method.

[0015] In the step S41, the treated 3D silk fiber structure is immersed in a LD-PEG precursor solution and irradiated under ultraviolet light for 2-5 minutes at a temperature of 35-40°C during swelling to obtain an LD-PEG hydrogel layer embedded with the 3D silk fiber structure.

[0016] In the step S42, the precursor solution of HD-PEG hydrogel is injected therein, and ultraviolet irradiation time is 2-5 minutes, and the swelling temperature is 35-40° C. to obtain a double-layer hydrogel scaffold.

[0017] To achieve the above objectives, a double-layer hydrogel scaffold for annulus fibrosus repair embedded with 3D silk fibers is designed for application in the field of annulus fibrosus repair and regeneration.

[0018] Compared with the prior art, the double-layer hydrogel scaffold obtained by the present invention has good adhesion, biocompatibility and mechanical strength. At the same time, by loading different cytokines, it is beneficial for bone marrow mesenchymal stem cells to differentiate into chondrocytes in the inner layer of the annulus fibrosus and fibroblasts in the outer layer, providing a favorable place for cell differentiation, and solving the problem that the differentiation and repair ability of seed stem cells in the hydrogel scaffold is weakened due to the influence of the microenvironment in the repair of the annulus fibrosus tissue engineering. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a process schematic diagram of the present invention.

[0020] Figure 2 Schematic diagram of the 3D silk fiber structure of the present invention Figure 1 .

[0021] Figure 3 Schematic diagram of the 3D silk fiber structure of the present invention Figure 2 . DETAILED DESCRIPTION

[0022] The present invention will be further described below with reference to the accompanying drawings.

[0023] like Figure 1As shown, the fiber ring repair double-layer hydrogel scaffold embedded with 3D silk fibers includes, from top to bottom, a HD-PEG hydrogel layer and a LD-PEG hydrogel layer, a 3D silk fiber structure is embedded in the LD-PEG hydrogel layer, the material of the HD-PEG hydrogel layer is 8-arm polyethylene glycol-norbornene, and the material of the LD-PEG hydrogel layer is 4-arm polyethylene glycol-norbornene.

[0024] like Figure 2 , Figure 3 As shown, the 3D silk fiber structure includes several layers of silk fiber structures, and each layer of silk fiber structure is distributed in an S-shape or a grid shape.

[0025] The material of the 3D silk fiber structure is one or more of natural silk, polylactic acid PLA, and polycaprolactone PCL.

[0026] The crosslink density has a significant effect on the mechanical properties, and the polyethylene glycol chemical substances are used in the present invention to control it, such as 4-arm vs. 8-arm and short-chain vs. long-chain. The use of two different polymers in two layers can minimize the interfacial adhesion problem, and the double or multi-layer PEG hydrogel can form a stable interface area to prevent delamination between different layers.

[0027] In the present invention, high-density polyethylene glycol (HD-PEG) will form the upper layer of the double-layer hydrogel, acting as a protective layer against mechanical stress; the bottom layer of the double-layer hydrogel will be prepared from low-density polyethylene glycol (LD-PEG) hydrogel, which has multiple functions, such as biodegradability, stem cell encapsulation, and promotion of stem cell differentiation into chondrocytes.

[0028] In addition, the 3D silk fiber structure has a strong interfacial bonding ability with the low-density polyethylene glycol hydrogel, and reinforcing materials such as fibers are introduced without changing the cross-linking density of the polymer network to enhance the stiffness of the hydrogel.

[0029] like Figure 1 As shown, the preparation method of the above-mentioned 3D silk fiber embedded fiber ring repair double-layer hydrogel scaffold comprises the following steps: S1, prepare HD-PEG hydrogel and LD-PEG hydrogel respectively; S2, preparing a 3D silk fiber structure: S21, pasting a number of ball steel pins on the PDMS mold according to a predetermined pattern to form a pile frame; S22, moving silk fibers around each pile to form a layer of silk fiber structure; S23, repeating step S22 to obtain a number of layers of silk fiber structure; S24, vertically stacking the several layers of silk fiber structure to form a 3D silk fiber structure; S3, treating the 3D silk fiber structure: S31, applying a silk fibroin solution on the 3D silk fiber structure, and subjecting the 3D silk fiber structure to a vacuum treatment so that the silk fibroin solution completely penetrates into the 3D silk fiber; S32, immersing the 3D silk fiber structure in ethanol to stabilize the structure of the silk fibroin coating, and removing the coating after drying to obtain a treated 3D silk fiber structure; S4, preparing a double-layer hydrogel scaffold: S41, immersing the treated 3D silk fiber structure in an LD-PEG precursor solution, vacuuming to remove air pockets in the 3D silk fiber structure, irradiating under ultraviolet light, swelling to an equilibrium state and then cutting to obtain an LD-PEG hydrogel layer embedded with the 3D silk fiber structure; S42, placing the LD-PEG hydrogel layer obtained in step S41 between two glass sheets, injecting the precursor solution of HD-PEG hydrogel therein, irradiating with ultraviolet light, separating from the glass sheet after photocrosslinking, and swelling to an equilibrium state in PBS to obtain a double-layer hydrogel scaffold.

[0030] The specific method of step S1 is as follows: S11, drying polyethylene glycol in a vacuum, dissolving the dried polyethylene glycol in a mixed solution and stirring at room temperature to obtain a mixture; S12, adding p-nitrophenyl chloroformate dropwise to the above mixture, activating and stirring under a nitrogen atmosphere, precipitating in cold ether and vacuum drying to obtain polyethylene glycol-norbornene.

[0031] In step S1, the polyethylene glycol selected for the HD-PEG hydrogel includes PEG8OH, and 8-arm polyethylene glycol-norbornene is prepared; the polyethylene glycol selected for the LD-PEG hydrogel includes PEG4OH, and 4-arm polyethylene glycol-norbornene is prepared.

[0032] In step S11, the mixed solution includes one or more of anhydrous dichloromethane, 4-dimethylaminopyridine, and trimethylamine, and the stirring time is 10-20 minutes to obtain a mixed solution.

[0033] In step S12, p-nitrophenyl chloroformate is added dropwise to the mixture, and the mixture is stirred continuously at room temperature for 20-28 hours, and polyethylene glycol-norbornene is obtained by cold ether precipitation method.

[0034] In step S41, the treated 3D silk fiber structure is immersed in a LD-PEG precursor solution and irradiated under ultraviolet light for 2-5 min at a temperature of 35-40°C during swelling to obtain an LD-PEG hydrogel layer embedded with the 3D silk fiber structure.

[0035] In step S42, the precursor solution of HD-PEG hydrogel is injected therein, and ultraviolet irradiation time is 2-5 minutes, and the swelling temperature is 35-40° C. to obtain a double-layer hydrogel scaffold.

[0036] The double-layer hydrogel scaffold obtained by the present invention has an upper layer HD-PEG hydrogel formed by high-density polyethylene glycol, which is prepared by 8-arm polyethylene glycol and polyethylene glycol diacrylate through thiol-norbornene photogelation; the lower layer LD-PEG hydrogel is formed by low-density polyethylene glycol, and a 3D silk fiber structure is embedded in the LD-PEG hydrogel, which is prepared by the same cross-linking chemical method using four-arm polyethylene glycol as a raw material. The 3D silk fiber structure is formed by fused deposition modeling (FDM), and the performance of the fiber can be controlled by adjusting various parameters during specific use. The double-layer hydrogel scaffold obtained by the present invention has multiple functions, such as biodegradability, stem cell encapsulation, and promotion of stem cell differentiation into chondrocytes. The double-layer hydrogel scaffold can load different cytokines, which is conducive to the directional differentiation of bone marrow mesenchymal stem cells into the inner layer chondrocytes and outer layer fibroblasts of the annulus fibrosus, providing a favorable place for cell differentiation, and solving the problem that the seed stem cells in the hydrogel scaffold are affected by the microenvironment and the differentiation and repair ability is weakened in the repair of the annulus fibrosus tissue engineering.

[0037] When used specifically, the fiber ring repair double-layer hydrogel scaffold embedded with 3D silk fibers obtained by the present invention is applied in the field of fiber ring repair and regeneration. When the present invention is used, a double-layer composite hydrogel loaded with cytokines (TGF-β1 / CTGF) is prepared, and the prepared double-layer composite hydrogel is blended with TGF-β1 / CTGF to obtain a double-layer composite hydrogel loaded with cytokines (physical embedding), and then the compatibility of BMSC and cytokine composite hydrogel scaffold is evaluated, and finally a practical test is carried out in the human body. The results show that the height of the human intervertebral disc is significantly improved, and the staining situation shows that the damaged fiber ring is effectively repaired, and the mechanical strength of the repaired fiber ring is good. Embodiment 1

[0038] The preparation method of the fiber ring repair double-layer hydrogel scaffold embedded with 3D silk fibers in this embodiment includes the following steps: S1: 5.007 g of dried PEG was dissolved in 20 mL of anhydrous dichloromethane (DCM) and dissolved with 2.504 g of 4-(dimethylamino)pyridine (DMAP) and 15.010 g of trimethylamine (TEA). The mixture was stirred at room temperature for 15 min and the hydroxyl groups of PEG were activated under a nitrogen atmosphere. Then, 25.009 g of p-nitrophenyl chloroformate (PNC) was added dropwise to the PEG solution and stirred at room temperature for 24 h under a nitrogen atmosphere. Subsequently, PEG-PNC was precipitated in cold ether. Vacuum-dried PEG-PNC was dissolved in 20 mL of DCM; 25.012 g of norbornene-methylamine solution (TCI) was added to the PEG-PNC solution diluted with 5 mL of DCM and incubated in the dark at room temperature for 6 h under a nitrogen atmosphere. Finally, PEG4NB or PEG8NB was collected by cold ether precipitation and dried in vacuum.

[0039] S2: Prepare a 3D silk fiber structure and coat it with a layer of silk solution so that it can maintain structural stability after being removed from the frame, and then undergo vacuum treatment to enhance the penetration of the silk solution into the silk fiber. This process was repeated twice, the first time using a 3 wt% silk solution and the second time using an 8 wt% silk solution. The 3D SF structure was then immersed in ethanol to stabilize the structure of the silk protein coating and finally dried and removed.

[0040] S3: The 3D silk fiber structure obtained after the above treatment was immersed in the LD-PEG precursor solution, which was then vacuumed to remove the air pockets in the 3D SF structure. It was then irradiated under ultraviolet light for 2 minutes, and finally the 3D SF / LD-PEG hydrogel was swollen to equilibrium in PBS (pH = 7.4) at 37°C and cut with a 4 mm biopsy punch.

[0041] S4: The 3D SF / LD-PEG hydrogel was placed between two glass slides, and the gap between the top of the hydrogel and the upper glass slide was adjusted to 0.2 mm by adjusting the height of the spacer. The precursor solution of the HD-PEG hydrogel was then injected into the gap, and then irradiated with UV light for 2 min. After photocrosslinking, the formed 3D SF / LD / HD hydrogel was carefully separated from the glass slide. Finally, the double-layer hydrogel was swelled to equilibrium in PBS (pH = 7.4) at 37°C to obtain a double-layer hydrogel scaffold A.

[0042] The 3D SF / LD / HD-PEG hydrogel A obtained in this example was tested for compressive stress-strain and shear storage modulus. First, we performed a compressive stress-strain test on the prepared 3D SF / LD / HD-PEG hydrogel A, and measured the compression modulus of the 3D SF / LD / HD-PEG hydrogel A to be 740±15KPa. In the unconstrained compression mode, the compression modulus of natural articular cartilage is 240-850KPa. It can be seen that 3D SF / LD / HD-PEG hydrogel A can be used as a biomaterial for cartilage replacement. Subsequently, the interfacial bonding force between HD-PEG and 3D SF / LD-PEG was evaluated, and the shear storage modulus test of 3D SF / LD / HD-PEG hydrogel A was performed. The results showed that when 10% strain was applied at a frequency of 60 times / min for 10 min, the shear storage modulus of 3D SF / LD / HD-PEG hydrogel A did not change, indicating that the interfacial bonding between the components was stable, and even after multiple twists, 3D SF / LD / HD-PEG hydrogel A remained stably bonded.

[0043] It can be seen from the above results that the double-layer hydrogel A obtained in this example has good adhesion and compressive stress resistance, and also has good biocompatibility, and can provide a good environment for cartilage formation. Embodiment 2

[0044] The preparation method of the fiber ring repair double-layer hydrogel scaffold embedded with 3D silk fibers in this embodiment includes the following steps: S1: 5.004 g of dried PEG was dissolved in 20 mL of anhydrous dichloromethane (DCM) and dissolved with 2.511 g of 4-(dimethylamino)pyridine (DMAP) and 15.025 g of trimethylamine (TEA). The mixture was stirred at room temperature for 15 min and the hydroxyl groups of PEG were activated under a nitrogen atmosphere. Then, 25.006 g of p-nitrophenyl chloroformate (PNC) was added dropwise to the PEG solution and stirred at room temperature for 24 h under a nitrogen atmosphere. Subsequently, PEG-PNC was precipitated in cold ether. Vacuum-dried PEG-PNC was dissolved in 20 mL of DCM; 25.010 g of norbornene-methylamine solution (TCI) was added to the PEG-PNC solution diluted with 5 mL of DCM and incubated in the dark at room temperature for 6 h under a nitrogen atmosphere. Finally, PEG4NB or PEG8NB was collected by cold ether precipitation and dried in vacuum.

[0045] S2: Prepare a 3D silk fiber structure and coat it with a layer of silk solution so that it can maintain structural stability after being removed from the frame, and then undergo vacuum treatment to enhance the penetration of the silk solution into the silk fiber. This process was repeated twice, the first time using a 4 wt% silk solution and the second time using a 9 wt% silk solution. The 3D SF structure was then immersed in ethanol to stabilize the structure of the silk protein coating and finally dried and removed.

[0046] S3: The 3D silk fiber structure obtained after the above treatment was immersed in the LD-PEG precursor solution, which was then vacuumed to remove the air pockets in the 3D SF structure. It was then irradiated under ultraviolet light for 2 minutes, and finally the 3D SF / LD-PEG hydrogel was swollen to equilibrium in PBS (pH = 7.4) at 37°C and cut with a 4 mm biopsy punch.

[0047] S4: The 3D SF / LD-PEG hydrogel was placed between two glass slides, and the gap between the top of the hydrogel and the upper glass slide was adjusted to 0.2 mm by adjusting the height of the spacer. The precursor solution of the HD-PEG hydrogel was then injected into the gap, and then irradiated with UV light for 2 min. After photocrosslinking, the formed 3D SF / LD / HD hydrogel was carefully separated from the glass slide. Finally, the double-layer hydrogel was swelled to equilibrium in PBS (pH = 7.4) at 37°C to obtain a double-layer hydrogel scaffold B.

[0048] The 3D SF / LD / HD-PEG hydrogel B obtained in this embodiment was tested for compressive stress-strain and shear storage modulus, respectively. First, we performed a compressive stress-strain test on the prepared 3D SF / LD / HD-PEG hydrogel B, and measured the compression modulus of 3D SF / LD / HD-PEG hydrogel B to be 725±14Kpa, which can be used as a biomaterial for cartilage replacement. Subsequently, the interfacial binding force between HD-PEG and 3D SF / LD-PEG was evaluated, and the shear storage modulus test of 3D SF / LD / HD-PEG hydrogel B was performed. The results showed that the shear storage modulus of 3D SF / LD / HD-PEG hydrogel B did not change when 10% strain was applied at a frequency of 60 times / min for 10 min, indicating that the interface binding between the components was stable, and even after multiple twists, 3DSF / LD / HD-PEG hydrogels were stably bound.

[0049] It can be seen from the above results that the double-layer hydrogel B of this embodiment has good adhesion and compressive stress resistance, and also has good biocompatibility, and can provide a good environment for cartilage formation. Embodiment 3

[0050] The preparation method of the fiber ring repair double-layer hydrogel scaffold embedded with 3D silk fibers in this embodiment includes the following steps: S1: 5.002 g of dried PEG was dissolved in 20 mL of anhydrous dichloromethane (DCM) and dissolved with 2.515 g of 4-(dimethylamino)pyridine (DMAP) and 15.041 g of trimethylamine (TEA). The mixture was stirred at room temperature for 15 min and the hydroxyl groups of PEG were activated under a nitrogen atmosphere. Then, 25.102 g of p-nitrophenyl chloroformate (PNC) was added dropwise to the PEG solution and stirred at room temperature for 24 h under a nitrogen atmosphere. Subsequently, PEG-PNC was precipitated in cold ether. Vacuum-dried PEG-PNC was dissolved in 20 mL of DCM; 25.003 g of norbornene-methylamine solution (TCI) was added to the PEG-PNC solution diluted with 5 mL of DCM and incubated in the dark at room temperature for 6 h under a nitrogen atmosphere. Finally, PEG4NB or PEG8NB was collected by cold ether precipitation and dried in vacuum.

[0051] S2: Prepare a 3D silk fiber structure and coat it with a layer of silk solution so that it can maintain structural stability after being removed from the frame, and then undergo vacuum treatment to enhance the penetration of the silk solution into the silk fiber. This process was repeated twice, the first time using a 2 wt% silk solution and the second time using a 6 wt% silk solution. The 3D SF structure was then immersed in ethanol to stabilize the structure of the silk protein coating and finally dried and removed.

[0052] S3: The 3D silk fiber structure obtained after the above treatment was immersed in the LD-PEG precursor solution, which was then vacuumed to remove the air pockets in the 3D SF structure. It was then irradiated under ultraviolet light for 2 minutes, and finally the 3D SF / LD-PEG hydrogel was swollen to equilibrium in PBS (pH = 7.4) at 37°C and cut with a 4 mm biopsy punch.

[0053] S4: The 3D SF / LD-PEG hydrogel was placed between two glass slides, and the gap between the top of the hydrogel and the upper glass slide was adjusted to 0.2 mm by adjusting the height of the spacer. The precursor solution of the HD-PEG hydrogel was then injected into the gap, and then irradiated with UV light for 2 min. After photocrosslinking, the formed 3D SF / LD / HD hydrogel was carefully separated from the glass slide. Finally, the double-layer hydrogel was swelled to equilibrium in PBS (pH = 7.4) at 37°C to obtain a double-layer hydrogel scaffold C.

[0054] The 3D SF / LD / HD-PEG hydrogel C obtained in this embodiment was tested for compressive stress-strain and shear storage modulus, respectively. First, we performed compressive stress-strain tests on the prepared 3D SF / LD / HD-PEG hydrogel C, and measured the compression modulus of 3D SF / LD / HD-PEG hydrogel C to be 716±14Kpa, which can be used as a biomaterial for cartilage replacement. Subsequently, the interfacial binding force between HD-PEG and 3D SF / LD-PEG was evaluated, and the shear storage modulus test of 3D SF / LD / HD-PEG hydrogel C was performed. The results showed that the shear storage modulus of 3D SF / LD / HD-PEG hydrogel C did not change when 10% strain was applied at a frequency of 60 times / min for 10 min, indicating that the interface binding between the components was stable, and even after multiple twists, 3DSF / LD / HD-PEG hydrogels were stably combined.

[0055] It can be seen from the above results that the double-layer hydrogel C obtained in this example has good adhesion and compressive stress resistance, and also has good biocompatibility, and can provide a good environment for cartilage formation.

[0056] Comparative Example 1: Compared with Example 1, in this embodiment, the 3D silk fiber three-dimensional fiber structure is not embedded in LD-PEG, and other conditions remain unchanged, and the final double-layer hydrogel has poor mechanical properties. The average compression modulus of the LD-PEG hydrogel was measured to be 15±3KPa, and the average compression modulus of the HD-PEG hydrogel was 700±5KPa. In the unconstrained compression mode, the compression modulus of natural articular cartilage is 240-850KPa. It can be seen that HD-PEG hydrogel can be used as a biomaterial for cartilage replacement, while the compression modulus of LD-PEG hydrogel is extremely low and cannot be used as a biomaterial for cartilage replacement.

[0057] Comparative Example 2: Compared with Example 1, in step 2 of this embodiment, the 3D silk fiber is not coated with the silk solution, and other conditions remain unchanged. The final 3D SF / LD / HD-PEG hydrogel structure is unstable and easily destroyed. The average compression modulus test of the uncoated 3D SF structure and the coated 3D SF structure was carried out. The results showed that the compression modulus of the coated 3D SF structure (563±6KPa) was significantly higher than that of the uncoated 3D SF structure (473±9KPa). In addition, after embedding 3D SF in LD-PEG, the fiber slippage is further prevented, resulting in the compression modulus of the final 3D SF / LD / HD-PEG hydrogel being higher than that of the coated 3D SF structure, indicating that the 3D SF three-dimensional fiber structure has advantages when used to enhance hydrogels.

[0058] Table 1 Properties of the double-layer hydrogel scaffolds obtained in Examples 1 to 3: Example Example 1 Example 2 Example 3 Material 3D SF / LD / HD-PEG 3D SF / LD / HD-PEG 3D SF / LD / HD-PEG Average compression modulus (KPa) 740±15 725±14 716±14 Table 2 Properties of the double-layer hydrogel scaffolds obtained from Comparative Examples 1 and 2: Example Comparative Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 2 Material LD-PEG HD-PEG 3D SF Coating 3D SF Average compression modulus (KPa) 15±3 700±5 473±9 563±6

Claims

1. A double-layer hydrogel scaffold for annulus repair embedded with 3D silk fibers, characterized in that: From top to bottom, it includes a HD-PEG hydrogel layer and a LD-PEG hydrogel layer. A 3D silk fiber structure is embedded in the LD-PEG hydrogel layer. The material of the HD-PEG hydrogel layer is 8-arm polyethylene glycol-norbornene, and the material of the LD-PEG hydrogel layer is 4-arm polyethylene glycol-norbornene.

2. The double-layer hydrogel scaffold for repairing annulus fibrosus embedded with 3D silk fibers according to claim 1, characterized in that: The 3D silk fiber structure comprises several layers of silk fiber structures, each layer of silk fiber structure is distributed in an S shape or a grid shape; the material of the 3D silk fiber structure is selected from one or more of natural silk, polylactic acid PLA, and polycaprolactone PCL.

3. A method for preparing a double-layer hydrogel scaffold for repairing annulus fibrosus embedded with 3D silk fibers, characterized in that: The steps include: S1, prepare HD-PEG hydrogel and LD-PEG hydrogel respectively; S2, preparing a 3D silk fiber structure: S21, pasting a number of ball steel pins on the PDMS mold according to a predetermined pattern to form a pile frame; S22, moving silk fibers around each pile to form a layer of silk fiber structure; S23, repeating step S22 to obtain a number of layers of silk fiber structure; S24, vertically stacking the several layers of silk fiber structure to form a 3D silk fiber structure; S3, treating the 3D silk fiber structure: S31, applying a silk fibroin solution on the 3D silk fiber structure, and subjecting the 3D silk fiber structure to a vacuum treatment so that the silk fibroin solution completely penetrates into the 3D silk fiber; S32, immersing the 3D silk fiber structure in ethanol to stabilize the structure of the silk fibroin coating, and removing the coating after drying to obtain a treated 3D silk fiber structure; S4, preparing a double-layer hydrogel scaffold: S41, immersing the treated 3D silk fiber structure in an LD-PEG precursor solution, vacuuming to remove air pockets in the 3D silk fiber structure, irradiating under ultraviolet light, and cutting after swelling to an equilibrium state to obtain an LD-PEG hydrogel layer embedded with the 3D silk fiber structure; S42, placing the LD-PEG hydrogel layer obtained in step S41 between two glass sheets, injecting the precursor solution of HD-PEG hydrogel therein, irradiating with ultraviolet light, separating from the glass sheets after photo-crosslinking, and swelling in PBS to an equilibrium state to obtain a double-layer hydrogel scaffold.

4. The method for preparing a double-layer hydrogel scaffold for repairing annulus fibrosus embedded with 3D silk fibers according to claim 3, characterized in that: The specific method of step S1 is as follows: S11, drying polyethylene glycol in a vacuum, dissolving the dried polyethylene glycol in a mixed solution and stirring at room temperature to obtain a mixture; S12, adding p-nitrophenyl chloroformate dropwise to the above mixture, activating and stirring under a nitrogen atmosphere, precipitating in cold ether and vacuum drying to obtain polyethylene glycol-norbornene.

5. The method for preparing a double-layer hydrogel scaffold for repairing annulus fibrosus embedded with 3D silk fibers according to claim 3 or 4, characterized in that: In the step S1, the polyethylene glycol selected for the HD-PEG hydrogel includes PEG8OH, and 8-arm polyethylene glycol-norbornene is prepared; the polyethylene glycol selected for the LD-PEG hydrogel includes PEG4OH, and 4-arm polyethylene glycol-norbornene is prepared.

6. The method for preparing a double-layer hydrogel scaffold for repairing annulus fibrosus embedded with 3D silk fibers according to claim 4, characterized in that: In the step S11, the mixed solution includes one or more of anhydrous dichloromethane, 4-dimethylaminopyridine, and trimethylamine, and the stirring time is 10-20 minutes to obtain a mixed solution.

7. The method for preparing a double-layer hydrogel scaffold for repairing annulus fibrosus embedded with 3D silk fibers according to claim 4, characterized in that: In the step S12, p-nitrophenyl chloroformate is added dropwise to the mixture, and the mixture is stirred continuously at room temperature for 20-28 hours, and polyethylene glycol-norbornene is obtained by cold ether precipitation method.

8. The method for preparing a double-layer hydrogel scaffold for repairing annulus fibrosus embedded with 3D silk fibers according to claim 3, characterized in that: In the step S41, the treated 3D silk fiber structure is immersed in a LD-PEG precursor solution and irradiated under ultraviolet light for 2-5 minutes at a temperature of 35-40°C during swelling to obtain an LD-PEG hydrogel layer embedded with the 3D silk fiber structure.

9. The method for preparing a double-layer hydrogel scaffold for repairing annulus fibrosus embedded with 3D silk fibers according to claim 3, characterized in that: In the step S42, the precursor solution of HD-PEG hydrogel is injected therein, and ultraviolet irradiation time is 2-5 minutes, and the swelling temperature is 35-40° C. to obtain a double-layer hydrogel scaffold.

10. Application of the double-layer hydrogel scaffold for annulus fibrosus repair embedded with 3D silk fibers as claimed in claim 1 or 3 in the field of annulus fibrosus repair and regeneration.

Citation Information

Cited By

  • Efficient amplification process and anti-aging application of human-derived amniotic mesenchymal stem cells

    CN120424867A